CHDM vs isosorbide: dosing heat-resistant copolyesters

Adding 1,4-cyclohexanedimethanol (CHDM) and isosorbide (ISB) to a polyester lets you tune glass transition, crystallinity and toughness on demand. In PET, CHDM reaches a toughness peak near 30 mol% while isosorbide raises Tg about 1.1°C for every 1 mol% added, about five times more efficient than CHDM. Keep isosorbide below 15 to 25 mol% if you need the resin to stay spinnable and semi-crystalline.

Why the dosage of CHDM and isosorbide decides copolyester performance

Formulating a heat-resistant copolyester usually means copolymerizing a rigid or cyclic diol into a PET or PCT backbone. The two diols people reach for most often are CHDM and isosorbide. Both interrupt the regular chain packing of the base polyester, which raises the glass transition temperature and suppresses crystallization. They do it at very different rates, and they pull mechanical properties in opposite directions.

The hard part is that the dosage to performance curves for these monomers are scattered across many separate polymer studies. A formulator who wants to know how much CHDM gives the best toughness, or how much isosorbide can be added before the fiber stops spinning, has to rebuild the curve from scratch each time. This article pulls those curves together for four copolyester families so the tradeoffs sit in one place.

What the data shows across four copolyester families

The numbers below come from copolymerization studies on PET, PCT and their derivatives. Each family was measured on its own baseline, so the absolute Tg of pure PET is not identical across tables. Read each table as internally consistent rather than cross-comparable.

PET modified with CHDM: a toughness parabola

Copolymerizing CHDM into PET from 0 up to 80 mol% produces three distinct responses.

CHDM contentGlass transition (Tg)Crystallinity stateElongation at break
0% (pure PET)76°Csemi-crystallineabout 5%
30 mol%about 83°Cfully amorphousabout 170%
50 mol%about 86°Cre-crystallizingabout 95%
75 mol%about 90°Ccrystallineabout 8%

The glass transition rises slowly and steadily. From 0 to 75 mol% CHDM, Tg climbs from 76°C to about 90°C, which is about 2°C per 10 mol% added. The cyclohexane ring in CHDM is softer than the benzene ring of the terephthalate unit but stiffer than the ethylene glycol segment, so the two effects roughly cancel and Tg nudges up gently.

Crystallinity behaves in the most interesting way. A small amount of CHDM disrupts the regular PET chain enough to kill crystallization: by 30 mol% the DSC melt peak disappears and the material becomes fully amorphous, which is also when transparency peaks. Push CHDM past 50 mol%, though, and the melt peak returns. At high concentration CHDM segments become ordered enough to crystallize on their own.

Toughness follows a near-perfect upside-down parabola. Pure PET breaks at about 5% elongation. At 30 mol% CHDM that number shoots up to about 170%, then collapses: about 95% at 50 mol% and only about 8% at 75 mol%, which is more brittle than the unmodified polymer. Tensile strength drifts down the whole time, from about 50 MPa to about 45 MPa.

The stereochemistry of CHDM matters too. Trans-CHDM outperforms the cis form. Across the range studied, crystallinity moved from about 22% to about 40% and tensile strength from about 39 MPa to about 43.6 MPa as the trans fraction rose. With a trans content of 68% to 80%, elongation at break reached as high as 190%.

The same logic carries to other polyester bases. In a CHDM-modified PEF-type resin, the toughness peak shifts right to about 60 mol% CHDM, where elongation climbs from about 5% to about 188%.

PEIT: isosorbide delivers efficient Tg growth

The PEIT family copolymerizes isosorbide (the ISB diol) into PET. Feeding isosorbide from 5% up to 80% gives an actual ISB copolymer content of about 3% to 44%, and the Tg response is strong.

ISB copolymer contentGlass transition (Tg)Note
3%76°Cfiber strength peaks
about 13%about 90°Cstrength falls back to PET level
23%about 102°Cspinnability fails
44%124°Ccannot be spun at all

Each 1 mol% of isosorbide raises Tg by about 1.1°C, taking the resin from 76°C to 124°C across the range. CHDM manages only about 0.2°C per mol%, so isosorbide is about five times more efficient at lifting Tg.

Mechanical strength rises first and then falls. Spun fibers at 3% ISB reached a breaking strength of 3.85 cN/dtex, about 45% above pure PET. Past 13% the strength slips below that of unmodified PET. Above 23% the melt stops spinning cleanly, and at 44% it cannot be spun at all.

There is a clear amorphous threshold. At 13% ISB the crystallinity drops from pure PET’s 19.3% to about 1.5%, and above 15% the copolyester is fully amorphous. The melting point follows, falling from 242°C to 217°C, and the melt peak vanishes above 23%.

One reassuring point for thermal stability: once isosorbide pushes the polymer fully amorphous above 15%, the thermal decomposition temperature is unaffected. The catch is molecular weight, which falls as ISB content rises because the secondary hydroxyl of isosorbide is less reactive and chain growth becomes harder.

PCT plus isosorbide: a Tg/Tm seesaw

In the PCT family (poly(cyclohexylenedimethylene terephthalate)), adding isosorbide drives a straight linear trade. Tg climbs and Tm falls in near-lockstep, like a seesaw.

ISB contentTgTmCrystallinity state
0% (pure PCT)93.9°C286.2°Csemi-crystalline
5.6%97°C279°Csemi-crystalline
10%100°C270°Csemi-crystalline
16%109°C263°Csemi-crystalline
20%111°C256°Csemi-crystalline
23.2%110.8°C243.9°Csemi-crystalline
25%117°C250°Csemi-crystalline
39%133°Cnoneamorphous
61%149°Cnoneamorphous

Per 1 mol% of isosorbide, Tg rises about 1.07°C and Tm drops about 2.1°C. Once ISB passes 25%, the melting point disappears entirely and the resin is amorphous.

Mechanically, more isosorbide means stiffer but more brittle. Tensile modulus rises from 1730 MPa at 16% ISB to 2140 MPa at 61%, while elongation at break collapses from 122% to 19%. Semi-crystalline samples that went through solid-state polymerization improved tensile strength from 44 MPa to 60 MPa.

Adding neopentyl glycol: a head-to-head comparison

A separate study held the base formulation constant and modified PET with three different diols at matched levels. This is the only table where the four resins sit on the same footing.

SampleThird diolTgTensile strengthElongation at breakLow-shear melt viscosity
Pure PETnone84°C33.8 MPa95%75 Pa·s
NPG variantNPG 1.2 mol80°C28.2 MPa49%23 Pa·s
CHDM variantCHDM 1.2 mol87°C25.8 MPa61%82 Pa·s
CHDM + ISB variantCHDM 7 + ISB 1.2 mol96°C41.1 MPa121%124 Pa·s

The counterintuitive finding: neopentyl glycol lowers Tg

Most formulators expect any rigid diol to push Tg up. Neopentyl glycol (NPG) breaks that intuition. At the same 1.2 mol addition level, NPG’s dimethyl structure actually increases chain flexibility, dropping Tg to 80°C, about 4°C below pure PET. NPG earns its place through melt flow and weather resistance, not through heat resistance. If your goal is a higher Tg, NPG is the wrong tool.

The dual-monomer combination is the real winner. The CHDM 7 mol plus ISB 1.2 mol sample beats pure PET on all three mechanical measures: higher Tg (96°C), higher strength (41.1 MPa) and higher elongation (121%). High CHDM supplies the toughness skeleton while isosorbide props up Tg at the rigid end. The cost is processability. Its melt viscosity reaches 124 Pa·s, about 5.4 times the NPG variant, though it does thin by about 34% under high shear. That means the processing window needs deliberate design, and in practice this is the detail formulators underestimate most.

Practical formulation rules

  • Target 25 to 35 mol% CHDM in PET when maximum toughness and transparency matter more than strength. Stay at or below 30 mol% to sit in the amorphous, toughest window.
  • Use isosorbide when you need Tg, not toughness. Budget about 1.1°C of Tg per 1 mol% of ISB, and expect brittleness to climb as you add more.
  • Keep isosorbide under 15 mol% if the product must stay semi-crystalline, and under about 23 mol% if you need to spin fibers. Past those points crystallization and spinnability collapse.
  • Reach for NPG when flow and weatherability are the priority, not heat resistance. It will lower Tg slightly.
  • Combine high CHDM with a small isosorbide dose when you want one resin that is both tough and heat resistant, then design the extrusion window around the higher melt viscosity.
  • Prefer trans-CHDM over cis when you can specify it. The trans isomer gives higher crystallinity and tensile strength and the best elongation.

Limitations you should keep in mind

These curves come from several independent copolymerization studies, each with its own base polymer, catalyst and molecular weight. The pure PET Tg is not identical across tables (about 76°C in one study, 84°C in another), so do not read the absolute numbers as a single continuous scale. The values are good starting windows for laboratory screening, not commercial recipes, and they should be re-validated on your own equipment with your own diol purity before any scale-up.

Bottom line

CHDM and isosorbide are complementary, not competing. CHDM buys toughness and transparency through an amorphous window centered near 30 mol%, while isosorbide buys Tg at about five times the efficiency. Neopentyl glycol is the odd one out: it improves flow and weathering but nudges Tg down. The strongest all-round resin in the data pairs high CHDM with a modest isosorbide dose, at the price of a narrower, more viscous processing window.

FAQ

How much CHDM should I add to PET for the best toughness?

The toughness of PET peaks at about 30 mol% CHDM, where elongation at break reaches roughly 170% compared with about 5% for pure PET. This is also the point where the resin becomes fully amorphous and most transparent. Adding more CHDM keeps raising Tg but makes the material brittle again, so 25 to 35 mol% is the practical sweet spot for toughness.

Why does CHDM make PET amorphous at 30% but crystalline again above 50%?

At low CHDM levels the irregular cyclohexane units disrupt PET’s regular chain packing, so crystallization stops and the polymer turns amorphous by about 30 mol%. Once CHDM concentration passes 50 mol%, the CHDM segments themselves become numerous and ordered enough to crystallize on their own, and the DSC melt peak reappears.

How efficiently does isosorbide raise the glass transition temperature?

Isosorbide is about five times more efficient than CHDM at lifting Tg. Each 1 mol% added to PET raises the glass transition by roughly 1.1°C, moving the resin from 76°C to 124°C across the studied range. CHDM manages only about 0.2°C per mol% over the same span. That is why isosorbide is the right diol when the only goal is a higher service temperature and the added brittleness is acceptable.

What is the spinnability limit for isosorbide in PEIT fibers?

Fibers spin cleanly up to about 13% isosorbide, where strength is still at or above pure PET. Spinnability starts to fail above 23% ISB and the material cannot be spun at all by 44%. Formulators targeting melt-spun fibers should keep isosorbide below roughly 20 mol% to stay safe. Above that limit the melt loses the cohesion needed for stable filament drawing, so the practical ceiling sits well under where Tg peaks.

At what isosorbide level does a copolyester become fully amorphous?

In PET-based PEIT, crystallinity falls to about 1.5% at 13% isosorbide and the resin is effectively fully amorphous above 15 mol%. In the PCT-based family the melting point disappears once isosorbide passes 25 mol%. The exact threshold depends on the base polymer, but 15 to 25 mol% is the usual amorphous window.

Why does neopentyl glycol lower Tg instead of raising it?

Neopentyl glycol has a dimethyl structure that increases local chain flexibility, so at a matched 1.2 mol addition it actually drops Tg to about 80°C, roughly 4°C below pure PET. Its value is in melt flow and weather resistance, not heat resistance. If you need a higher Tg, choose CHDM or isosorbide instead.

Which combination gives the best all-round copolyester?

The data points to high CHDM paired with a small isosorbide dose, specifically about 7 mol CHDM plus 1.2 mol ISB in the head-to-head study. That sample beat pure PET on Tg, tensile strength and elongation at once. The tradeoff is high melt viscosity, about 5.4 times the NPG variant, which demands a carefully designed processing window.

How does trans versus cis CHDM affect copolyester properties?

Trans-CHDM consistently outperforms the cis isomer. Raising the trans fraction from a low level toward 68% to 80% lifted crystallinity from about 22% to about 40% and tensile strength from about 39 MPa to about 43.6 MPa, while elongation at break reached as high as 190%. Specifying trans-rich CHDM is worth it when strength and toughness both matter.