A crosslinked PVC/polycarbonate (PVC-PC) nanofiltration membrane is made by bonding aromatic diamine groups onto PVC chains and then linking them to polycarbonate. The result is a three-dimensional polymer network that gets electrospun into nanofibers. In bench-scale testing, that membrane delivered roughly two and a half times the pure water flux of unmodified PVC, recovered more than 60% of its flux after protein fouling, removed 92 to 95% of lead, cadmium and arsenic, and rejected 93 to 98% of a broad set of pharmaceutical compounds.
Here is why that combination is worth attention. Treatment plants almost never face a single pollutant. Municipal and industrial streams carry dissolved salts, heavy metals and drug residues at the same time, and most membranes handle one of those well while letting the others through. What follows covers how this membrane is built, what the characterization data actually says, where it performs best, and where it falls short.
Why crosslink PVC with polycarbonate
Polyvinyl chloride is one of the most-used thermoplastics on earth. It is cheap, mechanically strong, resistant to chemicals and easy to process, which is why it shows up in pipes, medical devices, cable insulation and packaging. Those same traits make it a reasonable membrane material. It forms films easily, survives corrosive cleaning chemicals, and costs a fraction of the specialty polymers used in commercial nanofiltration.
The trouble is that PVC earns its low price by being chemically dull. Its surface is hydrophobic, it offers few functional groups for grabbing dissolved contaminants, and it fouls fast. Once proteins, colloids or organic matter settle on the surface, flux drops, cleaning cycles get more frequent, and service life shortens. Long-term dimensional stability is only moderate too.
Crosslinking fixes part of this by creating covalent bonds between polymer chains. Tie the chains together and their mobility drops. Mechanical strength, thermal stability, chemical resistance, solvent tolerance and dimensional stability all improve. Crosslinked PVC has already moved into water treatment membranes, medical devices, electrical insulation and engineering products on the strength of that.
Polycarbonate is the more interesting half of the pairing. It brings carbonate ester groups, aromatic rings, and much better thermal stability than PVC. Mixing the two physically is easy and unsatisfying. Without chemical bonding, the polymers tend to phase-separate, and the membrane ends up carrying the weaknesses of both instead of the strengths of either. The approach that works uses 1,4-benzenediamine (BDA) as a molecular bridge. One amine end displaces chlorine on the PVC backbone, and those amine groups then react with carbonate groups on the polycarbonate. What comes out is an interconnected network, not a blend.
How the membrane is made
The synthesis runs in two steps, and both of them matter to the final performance.
Attaching the diamine to PVC. PVC with a molecular weight around 90,000 g/mol is dissolved in dimethylformamide along with 1,4-benzenediamine and held under reflux at roughly 120 °C for about 12 hours. This is a nucleophilic substitution: amine groups on the diamine replace chlorine atoms along the PVC chain. The product is an amine-functionalized PVC intermediate.
Linking the polycarbonate. Polycarbonate, around 40,000 g/mol, is dissolved separately in DMF at about 60 °C and added dropwise to the PVC/BDA solution over roughly 30 minutes. Dibutyltin dilaurate goes in as a catalyst at about 1 wt% of total polymer mass. After an hour at room temperature to let the reactive groups find each other, the temperature goes back up to 120 °C for 24 hours under reflux. The polymer is then precipitated into excess ethanol, filtered, washed repeatedly, and dried under vacuum at 60 °C for 24 hours.
Electrospinning into nanofibers. The dried polymer is redissolved in DMF at 15 wt% and loaded into a syringe with a 0.7 mm stainless-steel needle. Spinning runs at 25 kV, a flow rate of 0.1 mL/h, and a tip-to-collector distance of 15 cm. Fibers land on a grounded rotating drum wrapped with a nonwoven polyester support, which gives uniform deposition and a defect-free layer. Four hours of spinning yields a membrane about 150 ± 10 μm thick, vacuum-dried at 60 °C for 12 hours to strip residual solvent.
Worth pausing on that last step. Electrospinning is an established industrial process, not a lab curiosity. A material that will not form continuous fibers is a material you cannot turn into a membrane, so the fact that this polymer spins cleanly, with no beads and no fiber breakage, says something real about scale-up.
What the characterization data shows
FT-IR confirms the chemistry
Infrared spectroscopy is where the chemical case gets made. Neat PVC shows what you would expect: C-H stretching near 2964 and 2941 cm⁻¹, C-C stretching at 1035 cm⁻¹, and the distinctive C-Cl stretch at 772 cm⁻¹.
After the diamine reaction, two new bands appear at 3651 and 3619 cm⁻¹ from N-H stretching, along with aromatic C=C bands at 1651 and 1617 cm⁻¹. That is direct evidence the diamine attached to the PVC backbone.
The more telling shift shows up once polycarbonate enters. The carbonate C=O stretch, which sits at 1778 cm⁻¹ in neat PC, moves down to 1723 cm⁻¹ in the crosslinked product. A 55 cm⁻¹ shift to lower wavenumber means the carbonyl bond order dropped, which points to hydrogen bonding between PC carbonyls and the N-H groups on the modified PVC, and possibly to urethane-like linkages formed with help from the catalyst. Either way, the polycarbonate is chemically or strongly physically tied into the PVC network instead of floating alongside it.
Elemental analysis puts numbers on it
Neat PVC is about 38% carbon. After diamine attachment, carbon climbs to roughly 62% and nitrogen reaches 10.3%, reflecting the added aromatic rings and amine groups. After crosslinking with polycarbonate, nitrogen collapses to 0.81% while oxygen comes in near 14% and residual chlorine sits at 7.2%.
Two things follow from that. The near-disappearance of nitrogen means the amine groups were consumed bonding to polycarbonate rather than left dangling. And the residual chlorine implies roughly 81% of the original chlorine atoms on the PVC were substituted, so crosslinking went a long way toward completion.
Thermal behavior improves
Neat PVC degrades in the familiar two-stage pattern: dehydrochlorination and HCl elimination around 220 to 320 °C, then breakdown of conjugated polyene structures. Polycarbonate holds up better, degrading mainly between 400 and 550 °C.
The crosslinked polymer gives a three-step profile. PVC dehydrochlorination shifts up to 250 to 320 °C, diamine-derived segments break down at 350 to 450 °C, and PC structural units go at 480 to 600 °C. The PVC degradation range moving to higher temperature is the part that matters, because the network is shielding the PVC backbone.
DSC adds a compatibility check. Instead of two separate glass transitions, the crosslinked material shows one broad transition spanning roughly 90 to 130 °C. A single broad Tg means the two polymers are integrated at the molecular level. The breadth reflects uneven crosslink density through the network, which is normal for this kind of reaction.
Swelling, and what Flory-Huggins says about it
Swelling data explains why the membrane moves water as well as it does. Over four hours in water, neat PVC goes from 1.4% to just 1.6%, which is essentially nothing. The crosslinked PVC-PC climbs from 3.9% to 6.2% and has not leveled off yet.
Run those numbers through Flory-Huggins theory and you get a polymer volume fraction of 0.984 for PVC against 0.942 for PVC-PC. The modified network holds about four times more water, a volume fraction of 0.058 versus 0.016. The interaction parameter falls from 3.255 for PVC-water to 2.147 for PVC-PC-water, so the modified polymer is thermodynamically friendlier to water.
Both values stay far above the 0.5 threshold that marks a good solvent, so water remains a poor solvent for this material and swelling stays limited. That is what you want. Enough affinity to sustain flux, not so much that the structure loosens and selectivity goes with it.
Performance: flux, fouling and contaminant rejection
Water flux
Pure water flux was measured in a dead-end cell with a 12 cm² active area, after 30 minutes of compaction at 1 bar. Between 1 and 5 bar, the crosslinked PVC-PC membrane delivered 65.34 to 93.36 L/m²·h. Unmodified PVC managed 27.68 to 38.96 L/m²·h over the same range.
Call it a 2.5-fold gain. It lines up with the swelling and Flory-Huggins results: more free volume and better water affinity mean lower hydraulic resistance. The near-linear rise in flux with pressure also tells you the membrane holds its shape under load instead of compacting.
Antifouling behavior
Fouling was tested with bovine serum albumin at 1 g/L, pH 7, 25 °C and 1 bar, cycling through pure water filtration, protein filtration, a 20-minute rinse and an overnight soak.
The numbers:
- Flux recovery ratio: 63.87% for PVC-PC against 39.77% for pristine PVC
- Reversible fouling: 12.25% against 4.84%
- Irreversible fouling: still high at 69.95%
The gain in flux recovery is real, and the rise in reversible fouling is good news too, because a larger share of the protein deposit is loosely attached and rinses away. The honest caveat sits in that third number. This membrane fouls less than unmodified PVC, but at roughly 70% irreversible fouling it is not a low-fouling membrane in the way a properly hydrated hydrophilic surface would be.
Salt rejection
Rejection was tested against NaCl, Na₂SO₄, MgCl₂, MgSO₄, CaCl₂ and CaSO₄ at 500, 1000 and 2000 ppm and 1 bar, and it rises as feed concentration rises. Two mechanisms are in play. The hydrophilic groups introduced by crosslinking interact more strongly with salt ions. On top of that, at higher concentrations partial pore clogging and surface fouling also push the measured rejection up.
That second one deserves a flag. Rejection that partly comes from fouling is not stable rejection. For process design, it means specifying this membrane with some margin rather than at the edge of its measured numbers.
Heavy metal removal
Lead, cadmium and arsenic removal was tested from 500 to 2500 ppm. Removal improves with concentration, up to a point:
| Feed concentration | As | Cd | Pb |
| 2000 ppm | 95% | 92% | 92% |
| 2500 ppm | 91% | 88% | 87% |
The climb from 500 to 2000 ppm comes from a steeper concentration gradient driving mass transfer toward the membrane surface and more contact with the hydrophilic functional groups. Past 2000 ppm, performance drops because adsorption sites saturate, and concentration polarization plus surface fouling pile rejected ions against the membrane wall, cutting the effective driving force.
Pressure matters even more. Raising transmembrane pressure from 0.5 to 5 bar dropped rejection from 97% to 66% for arsenic, 95% to 68% for cadmium, and 93% to 65% for lead. Low pressure means longer residence time, which favors adsorption and surface complexation. High pressure pushes permeate through faster, shortens contact time, and intensifies concentration polarization.
So the operating rule is simple enough: moderate feed concentration and low pressure give the best heavy metal removal. Chase throughput with pressure and you pay for it in rejection.
Pharmaceutical removal
This is where the crosslinked membrane puts the most distance between itself and plain PVC. Across 20 structurally diverse drugs, the PVC-PC membrane hit 93 to 98% rejection while pristine PVC managed 68 to 75% on the same set. The compounds covered beta-lactams (ampicillin, amoxicillin, penicillin G, ticarcillin), fluoroquinolones (ciprofloxacin), proton pump inhibitors (pantoprazole, omeprazole), and larger therapeutic agents.
The mechanism works on two levels. First, interfacial retention: polar groups on the modified membrane form hydrogen bonds, van der Waals forces and electrostatic interactions with the hydrophilic parts of drug molecules, the -NH, -COO- and C=O sites. Unmodified PVC is too hydrophobic to do much of that. Second, size exclusion. Pharmaceuticals tend to be bulky, multi-ring and rigid, and the tighter pore architecture of the crosslinked membrane blocks them physically, where the larger effective pores of pristine PVC let more through.
Rejection held above 93% across every drug class tested, which suggests the mechanism does not depend on one specific chemical interaction. For a plant facing an unpredictable mix of pharmaceutical residues, that consistency across the board is worth more than a higher number on a single compound.
How it stacks up against existing options
Measured against published benchmarks, the crosslinked PVC-PC membrane does well. Commercial nanofiltration membranes and polyamide thin-film composites reach high rejection on individual pharmaceuticals, sometimes above 97%, but rarely across heavy metals and pharmaceuticals in one material. Adsorptive composites like PVC/ZnO get high ciprofloxacin rejection. Various cellulose acetate and PVC/graphene oxide formulations handle specific metals well.
What sets this one apart is range without complexity. It covers two very different contaminant classes at high efficiency without embedding nanoparticles or running a multi-step fabrication. Both of those push up cost and complicate manufacturing, so skipping them counts for something when you think about scale.
Where it fits, and what still needs work
The realistic uses are municipal wastewater polishing where drug residues are a concern, industrial effluent with mixed metal contamination, and pre-treatment ahead of reverse osmosis, where fouling control and stable flux take load off the downstream units. PVC’s low material cost helps in all three.
The limits are worth saying plainly. Irreversible fouling near 70% is high. Long-term stability under real feedwater, with its swinging pH, competing organics and biological activity, has not been established. Performance shifts noticeably with pressure and concentration, so the operating window has to be respected. And this is bench-scale work.
Where does it go next? Optimize the polymer composition and the electrospinning parameters, attack the irreversible fouling component directly, and validate against real wastewater rather than single-solute laboratory solutions.
Key takeaways
- Crosslinking PVC with polycarbonate through an aromatic diamine produces a chemically bonded network, confirmed by FT-IR peak shifts and elemental analysis showing about 81% chlorine substitution.
- The modified membrane holds roughly four times more water than unmodified PVC and interacts with water more favorably, with a Flory-Huggins interaction parameter of 2.147 against 3.255.
- Pure water flux reaches 65 to 93 L/m²·h between 1 and 5 bar, about 2.5 times unmodified PVC.
- Flux recovery after protein fouling improves from 39.77% to 63.87%, although irreversible fouling stays high.
- Heavy metal removal peaks at 92 to 95% at 2000 ppm and low pressure, then falls off with either higher concentration or higher pressure.
- Pharmaceutical rejection reaches 93 to 98% across 20 compounds, against 68 to 75% for unmodified PVC.
Frequently asked questions
What is a crosslinked PVC-PC nanofiltration membrane? A filtration membrane made from polyvinyl chloride chemically bonded to polycarbonate through an aromatic diamine crosslinker, then electrospun into nanofibers. The crosslinking creates a three-dimensional polymer network that is more hydrophilic, more thermally stable and more permeable than unmodified PVC.
Why crosslink instead of just blending PVC and polycarbonate? Blending tends to produce phase separation, so the material inherits the weaknesses of both polymers. Crosslinking forms covalent bonds between chains, which improves mechanical strength, thermal stability, chemical resistance and dimensional integrity while adding the functional groups needed to interact with contaminants.
How much does crosslinking improve water flux? Pure water flux went from 27.68 to 38.96 L/m²·h for unmodified PVC up to 65.34 to 93.36 L/m²·h for the crosslinked membrane across the same 1 to 5 bar range, roughly a 2.5-fold improvement.
Can this membrane remove pharmaceutical residues from water? Yes. It rejected 93 to 98% of 20 structurally diverse pharmaceutical compounds, including beta-lactam antibiotics, fluoroquinolones and proton pump inhibitors, against 68 to 75% for unmodified PVC.
What operating conditions give the best heavy metal removal? Moderate feed concentration near 2000 ppm combined with low transmembrane pressure around 0.5 bar. Removal drops at higher concentrations because adsorption sites saturate, and drops at higher pressures because shorter contact time and stronger concentration polarization reduce ion retention.
Is the membrane fully fouling resistant? No. Flux recovery improves substantially, from 39.77% to 63.87%, and more of the fouling becomes reversible, but irreversible fouling still accounts for roughly 70%. It resists fouling better than unmodified PVC rather than eliminating it.
Is this technology ready for industrial deployment? It is at bench scale. Material costs are favorable and fabrication uses established electrospinning equipment, but long-term stability under real feedwater and scale-up behavior still need to be demonstrated.