Hydrophobic Polypropylene at 124.9 Deg, 26x Tougher

PP melt blending with 6 wt% of a long-chain alkyl fluorinated polysiloxane gets you both properties at once. At a monomer ratio of 1:1:0.06 (D4 to D3F to hexadecyltrimethoxysilane), the water contact angle hits 124.92 degrees against 105 degrees for neat PP. That is what hydrophobic polypropylene looks like in practice. Toughness goes from 6.1 to 164.3. Elongation at break passes 800%. And the whole thing compounds on ordinary equipment at ordinary temperatures.

Why hydrophobic polypropylene usually trades away toughness

Polypropylene is everywhere for boring, good reasons. It is cheap, light, resistant to most chemicals you would care about, and it runs through a moulder without complaint. Two weaknesses keep it out of better jobs. Its surface sits at a water contact angle near 105 degrees, which is water resistant in the everyday sense and useless for anything that needs self cleaning, anti icing, or anti fouling behaviour. And it is brittle where it counts: cold, or under impact, or at a notch.

The standard fixes fight each other. Fluorinated low surface energy additives migrate outward and lift the contact angle, but they get along badly with PP, so they clump, and every clump is a place for a crack to start. Elastomer tougheners such as POE or EPDM do the reverse. They fix impact and leave the surface exactly as wettable as before, and they usually take stiffness with them. Doing both at once is not a mixing problem, it is a compatibility problem wearing a mixing problem’s clothes. That is the real obstacle in PP modification, and it is why so many hydrophobic PP composite trials stall at the plaque stage.

Two ideas carry most of the published work on polypropylene toughening. One is Cassie-Baxter: pair low surface energy chemistry with a rough surface, trap air in the texture, and let the droplet sit on a composite of solid and air. The other is the interpenetrating polymer network, or IPN, where two networks entangle instead of reacting, so stress crosses a tight interface rather than piling up at a weak one. The study this article walks through tries to get both from one additive. That is the interesting part.

I want to be upfront about the framing here. This is a laboratory study with a laboratory mixer and compression moulded plaques. It is not a datasheet, and none of these numbers should go into a part drawing unverified. What it does offer is a rare side by side look at three formulation variables moved independently, which is more useful than another single point optimisation.

The three formulation levers in hydrophobic polypropylene modification

Here is the map before the territory. Three variables were moved, and the results refuse to line up with the assumption that more additive means more effect.

LeverWhat it controlsRange testedWhat the data showed
D4 to D3F molar ratioBalance between siloxane flexibility and fluorine content2:1, 1.5:1, 1:1, 1:1.5, 1:21:1 gave the best hydrophobicity. Pushing fluorine to 1:2 or diluting it to 2:1 both cost toughness.
Hexadecyltrimethoxysilane levelCompatibility of the modifier with the PP matrix0.02 to 0.10 molar, against a 1:1 D4 to D3F base0.06 gave the best combined result. 0.02 stretched furthest but gave up stiffness.
Modifier loading in the compoundHow much modifier reaches the surface versus staying in the bulk2 to 10 wt%6 wt% was the peak. 4 and 8 wt% were both clearly worse, and the response is not monotonic.

That last row is the one to internalise. If your screening plan assumes a straight line between loading and performance, this system will hand you a confident wrong answer.

Building the modifier: one pot, ring-opening polymerization

The additive is a long-chain alkyl fluorinated polysiloxane, labelled FPW C16 X throughout, where X tracks the monomer ratio. Three monomers go into an anionic ring-opening polymerization.

Octamethylcyclotetrasiloxane, D4, supplies the dimethylsiloxane backbone and with it the flexibility and thermal stability. D3F, which is 1,3,5 trimethyl 1,3,5 tris(3,3,3 trifluoropropyl)cyclotrisiloxane, carries the trifluoropropyl groups that do the surface work. Hexadecyltrimethoxysilane, sold as Dynasylan 9116, contributes the C16 chain that makes the whole molecule tolerable to polypropylene.

The catalyst is a tetramethylammonium hydroxide alkali gum at 0.01 wt%. The charge goes to 120 degrees Celsius for 2 hours, clears, and is then stripped at 175 degrees Celsius under roughly 0.1 MPa of reduced pressure to pull off low boilers. Out comes a transparent viscous fluid. The 1:1:0.06 batch produced 35.81 g at 91.14% yield, which is a healthy number for a siloxane equilibration.

ParameterValue
MonomersD4, D3F, hexadecyltrimethoxysilane
CatalystTetramethylammonium hydroxide alkali gum, 0.01 wt%
Polymerization120 degrees Celsius for 2 hours
Stripping175 degrees Celsius at about 0.1 MPa reduced pressure
Product formTransparent viscous fluid, 91.14% yield for the 1:1:0.06 grade
Number average molecular weight7,849
Weight average molecular weight16,997
Z average molecular weight31,618
Polydispersity index2.1
Compounding10 min premix at 100 degrees Celsius, then 20 min at 180 degrees Celsius in an internal mixer
MoldingCompression molding at 180 degrees Celsius

What the characterization actually proved

Three techniques were used and they agree, which is more than you can say for a lot of additive papers.

FTIR shows the sharp cyclic Si O Si bands of the D4 and D3F monomers at 1080 and 1020 per cm vanishing, replaced by a broadened Si O Si band between 1050 and 1080 per cm. That is what ring opening into linear chains looks like. A CF3 band sits at 1214 per cm as a split multiplet, and C F stretching from 1200 to 1300 per cm coexists with C H stretching at 2850 to 2960 per cm. Fluoroalkyl and long-chain alkyl are both present.

Proton NMR found no residual cyclic monomer between 0.1 and 0.3 ppm, so the rings opened completely. Methyl protons next to silicon land at 0.02 to 0.04 ppm, the terminal methyl of the C16 chain at 0.61 to 0.63 ppm, long chain methylenes near 1.17 ppm, the methylene next to the siloxane backbone on the fluoroalkyl side near 1.96 ppm, and the methylene adjacent to CF3 at 3.36 to 3.40 ppm. Fluorine 19 NMR gives a single peak at minus 68.86 ppm, assigned to the CF3 of the trifluoropropyl group. Silicon 29 NMR puts the linear structure signal between minus 21 and minus 23 ppm.

GPC gave one symmetric peak with a polydispersity of 2.1. No leftover monomer, no high molecular weight tail.

How much hydrophobic and how much tough does the compound actually get?

The headline figures come from the 1:1:0.06 modifier at 6 wt%.

PropertyNeat PPBest modified compoundChange
Water contact angle105 degrees124.92 degrees+18.97%
Toughness6.1164.325.93 fold, as reported
Elongation at break23.9%804.6%About 34 fold
Tensile strength36.5 MPa27.5 MPaDown 24.6%
Elastic modulus1,144.0 MPa962.4 MPaDown 15.9%
Temperature at 5% mass loss370 degrees Celsius365 degrees CelsiusDown 5 degrees
Temperature at max loss rate490 degrees Celsius461 degrees CelsiusDown 29 degrees

Read it honestly. The elongation and toughness gains are enormous, and they are bought with stiffness and strength. This is a toughening route, not a reinforcing route. Anyone who specs it into a load bearing part without rechecking the modulus is going to have a bad week.

Molar ratio results

D4 : D3F : silaneTensile strength (MPa)Elongation at break (%)Elastic modulus (MPa)Toughness
Neat PP36.523.91,144.06.1
1 : 1 : 0.0232.01,131.5624.7322.0
1 : 1 : 0.0439.0752.61,418.1217.4
1 : 1 : 0.0627.5804.6962.4164.3
1 : 1 : 0.0828.4824.81,105.1191.5
1 : 1 : 0.1026.6660.8606.6138.9
2 : 1 : 0.0622.2554.01,024.1101.5
1.5 : 1 : 0.0626.4733.11,044.3165.3
1 : 1.5 : 0.0627.5866.7889.6220.0
1 : 2 : 0.0622.7695.8887.8125.4

Loading level results for the 1:1:0.06 modifier

Loading (wt%)Tensile strength (MPa)Elongation at break (%)Elastic modulus (MPa)Toughness
036.523.91,144.06.1
229.8780.9895.2164.0
430.2333.51,156.072.0
627.4804.6962.4164.3
826.0450.11,162.488.8
1026.7666.3953.6137.3

Thermal stability: what you give up

Thermogravimetric analysis puts a number on the cost. Adding the modifier is not free. Neat PP reaches 5% mass loss at 370 degrees Celsius and peaks at 490 degrees Celsius. The 1:1:0.06 compound comes in at 365 and 461. The 1:1.5:0.06 grade drops further, to 330 and 458.1. Derivative peak positions stay within 5 degrees across the whole series, so the degradation mechanism has not changed. It just starts a little sooner.

That is a smaller penalty than most people assume for a silicone additive for PP, and the reason is structural. The Si O Si backbone is thermally more robust than a carbon backbone, and the C F bond is among the strongest single bonds in organic chemistry. The earlier mass loss most likely comes from the C16 chain and any residual low boilers, not from the siloxane. Processing sits at 180 degrees Celsius, far below all of this. There is headroom.

DSC found a single melting peak for every compound, which is a compatibility signal worth having. Two peaks would mean two badly mixed phases pretending to be one material.

Crystallinity fell slightly, from 29.5% for neat PP to 29.3% for the 1:1:0.06 compound and 28.9% for 1:1.5:0.06. Small numbers, real consequences. Less crystallinity means a larger amorphous fraction, and amorphous regions let chain segments move, which is how energy gets absorbed instead of driving a crack across the part.

Why the surface sheds water: roughness plus low surface energy

AFM separates the two contributions cleanly. The 1:1:0.06 compound measures 119 nm RMS roughness and 95.1 nm average, against 65.3 and 52.8 nm for neat PP. Roughness nearly doubled, so by the Cassie-Baxter model, air gets trapped in the texture and the apparent contact angle climbs.

Then there is the sample that spoils the tidy story. The 1:1.5:0.06 compound came out smoother than neat PP, 21.6 nm RMS and 17.1 nm average, and it still behaved hydrophobically. Roughness alone cannot account for that. The fluorine does the work by itself. For anyone designing a part that will see abrasion, this is the more useful finding of the two: a texture dependent surface stops working the moment the texture wears off, while a chemistry dependent one keeps working until the surface layer is gone.

What DMA and rheology say about the mechanism

DMA tracks storage modulus, the elastic response, against loss modulus, the viscous response. Both fall as temperature rises, as they always do. The modified compounds start lower than neat PP at room temperature, and 1:1:0.06 starts lowest of all. Lower here means less internal friction across the normal service range, which is what toughness feels like from the inside. The modified curves also decay more slowly at high temperature, so the material holds shape better when hot.

The loss factor curve says it most clearly. Lower tan delta means better toughness, and the modified curve shifts right, toward higher temperature. A rightward shift is a delayed phase transition, in plain terms a higher glass transition temperature. The flexible Si O Si segments and the C16 chains make the compound easier to deform when cold, while the high bond energy C F groups and the entangled network hold it together when hot. The authors call this low temperature plasticization paired with high temperature reinforcement, and the DMA storage modulus and tan delta data support them.

Rheology agrees. At matched angular frequency, 1:1:0.06 shows the highest storage modulus in the series, so it resists instantaneous deformation best and has the best dynamic stability. That is the entangled network doing its job, transferring stress rather than letting chains slide. The same compound also has the highest loss modulus, meaning it dissipates the most energy. High storage modulus together with high loss modulus is exactly what you want in something that has to stay dimensionally stable and damp vibration at the same time, such as automotive damping components or electronic packaging exposed to high frequency loading.

Fracture morphology: reading the broken surface

Neat PP breaks in a layered, lamellar pattern. Textbook brittle fracture.

The compounds look nothing like it. Their fracture surfaces are rough, covered in linear stress marks and river like striations, with visible crack deflection.

Those river patterns are the mechanism made visible. A crack running into the IPN forks into secondary cracks instead of going straight through. Every fork lengthens the path and increases the fracture surface area, so more energy is absorbed before the part separates. Smooth and layered is what you get when a crack runs along a weak interface with nothing in its way.

TEM shows the same thing from inside. Neat PP looks continuous and flat. The compounds show partially disordered crystalline patterns with lighter, sea island regions embedded in the matrix. Those islands interfere with PP crystallization, and a less ordered structure tolerates deformation better. This matches the small crystallinity drop measured by DSC, which is reassuring.

The counterintuitive part

Three results here cut against normal compounding intuition.

One formulation got stronger and stiffer and tougher at the same time. The 1:1:0.04 compound measured 39.0 MPa tensile strength and 1,418.1 MPa modulus, both above neat PP’s 36.5 and 1,144.0, while elongation went from 23.9% to 752.6% and toughness from 6.1 to 217.4. Strength, stiffness, and toughness moving up together is not supposed to happen. It happened here. If you only read the headline 1:1:0.06 result, you would never see it.

The best toughness number lost. The 1:1:0.02 grade reached 1,131.5% elongation and 322.0 toughness, roughly double the toughness of the formulation the authors selected as best overall. It lost on contact angle and stiffness. Pick a formulation on one metric in this system and you will pick wrong.

Loading is not a dial. Two wt% gave 164.0 toughness, four gave 72.0, six gave 164.3, eight gave 88.8, and ten recovered to 137.3. There is a window around 6 wt% and it is ringed by worse results on both sides. Any scale up plan needs tight control of the loading level, because a two point drift can halve the property you are paying for.

Practical takeaways for compounders

  • Start screening at 6 wt% and treat 4 and 8 wt% as failure points rather than points on a curve. Behaviour near the optimum is not linear.
  • Decide early whether you are optimising for hydrophobicity or for PP toughness, because the best formulation differs. The 1:1:0.02 grade wins on elongation, 1:1:0.06 wins on contact angle, and 1:1:0.04 is the only one that beats neat PP on strength and stiffness.
  • Budget for roughly 16% modulus loss and roughly 25% strength loss at the headline formulation. If the part is stiffness critical, look at 1:1:0.04 instead.
  • Do not assume you need surface texture. A fluorine bearing modifier can deliver hydrophobicity on a smooth surface, and that survives wear far better than texture does.
  • Check the thermal window before committing. Processing at 180 degrees Celsius is safe, but degradation onset moves 5 to 40 degrees earlier depending on grade.
  • Treat fluorinated additives as a compliance question, not only a technical one. PFAS rules are moving quickly in several markets, and a trifluoropropyl functional siloxane deserves a PFAS regulatory review before it reaches a commercial product.
  • Reprocessing and recyclability were not evaluated. If the part enters a recycle stream, test it.

Limitations

Single study, single injection molding grade of PP, one modifier at one molecular weight, Mn 7,849. None of this transfers automatically to a different PP grade or a different siloxane chain length.

Toughness is reported as the area under the stress strain curve, in J per cubic metre. The reported fold change of 25.93 does not match the raw ratio of 164.3 to 6.1 exactly, and the discrepancy is not explained. Treat the fold change as approximate.

Contact angles are static, taken with 5 microlitre droplets at three spots per sample following ISO 15989. No sliding angle, no roll off, no abrasion testing, no weathering. A static contact angle says a droplet beaded up once. It says nothing about year two outdoors, or about wipe number one hundred.

Mechanical testing followed GB/T 1040.1 at 30 mm per minute, one strain rate. Impact strength, which is what most engineers actually specify against, was never measured. Eight hundred percent elongation at break is not a notched Izod number and should not be read as one.

All compounding was done in a laboratory internal mixer with compression moulding afterwards. Extrusion and injection molding impose different shear and cooling histories, and both influence where the modifier ends up in a finished part.

Bottom line

A long-chain alkyl fluorinated polysiloxane built from D4, D3F, and hexadecyltrimethoxysilane at 1:1:0.06, added at 6 wt%, takes polypropylene from 105 degrees to 124.92 degrees water contact angle and multiplies toughness roughly 26 fold. Low surface energy chemistry handles the surface, an interpenetrating network handles the bulk. The bill is about 16% of elastic modulus, about 25% of tensile strength, and a small shift in degradation onset. Where water shedding and impact tolerance matter more than rigidity, that is a trade worth making.

FAQ

What is hydrophobic polypropylene?

Hydrophobic polypropylene is PP whose surface has been modified so water beads up instead of spreading. Unmodified PP sits at about 105 degrees water contact angle, which is only mildly water resistant. A hydrophobic grade pushes past 120 degrees, usually by adding a low surface energy additive that migrates to the surface, by texturing the surface, or by doing both at once.

How do you make polypropylene hydrophobic and tough at the same time?

The route tested here melt blends a long-chain alkyl fluorinated polysiloxane into PP at 6 wt%. The fluorinated groups lower surface energy and raise the water contact angle, while the flexible siloxane backbone and C16 alkyl chain form an interpenetrating network that absorbs energy. Both effects come from one additive, which avoids the compatibility problems of separate packages.

What water contact angle counts as hydrophobic for polypropylene?

Neat polypropylene measures about 105 degrees. Anything above 90 degrees is technically hydrophobic, but most functional targets start at 120 degrees. The formulation discussed here reached 124.92 degrees, an 18.97% improvement over neat PP. Superhydrophobic status needs 150 degrees or more plus a low sliding angle, which this system does not reach.

How much modifier is needed to toughen polypropylene in this system?

Six percent by weight was the optimum, and the response around it is not linear. At 2 wt% toughness reached 164.0, at 4 wt% it fell to 72.0, at 6 wt% it was 164.3, at 8 wt% it dropped to 88.8, and at 10 wt% it recovered to 137.3. A two point drift away from 6 wt% can halve the result. That is why tight control of the loading level matters when the formulation is scaled up.

Why add a long-chain alkyl group to a fluorinated polysiloxane?

The C16 alkyl chain is a compatibility handle. Fluorinated siloxanes and polypropylene are poorly matched, and without a compatibilizing segment the modifier agglomerates, creating stress concentrators that cancel out the toughening. Grafting a long alkyl chain onto the siloxane lets it entangle with PP chains, so the modifier disperses and the interface holds under load.

Does the polysiloxane modifier hurt the thermal stability of polypropylene?

Slightly. Neat PP reaches 5% mass loss at 370 degrees Celsius and peaks at 490 degrees Celsius. The 1:1:0.06 compound sits at 365 and 461 degrees Celsius, and the 1:1.5:0.06 grade at 330 and 458.1 degrees Celsius. Peak positions shift by no more than 5 degrees, so the mechanism is unchanged. Processing at 180 degrees Celsius is unaffected.

What is an interpenetrating polymer network in PP toughening?

An interpenetrating polymer network, or IPN, is a structure where two polymer networks are entangled rather than covalently bonded, giving strong interfacial contact in all directions. In PP toughening it matters because stress transfers across the interface instead of concentrating at a weak boundary. Cracks that meet the network fork into secondary cracks and absorb more energy before the part fails.

Does hydrophobicity require a rough surface?

No, and this work is a clean demonstration. The 1:1:0.06 compound had a roughness of 119 nm RMS and a high contact angle, which fits the Cassie-Baxter air trapping model. But the 1:1.5:0.06 compound was smoother than neat PP at 21.6 nm RMS and still repelled water, because the fluorinated groups alone lowered the surface energy enough.

Is a higher water contact angle always better for polypropylene?

Not on its own. The formulation with the best toughness in this study, at 1:1:0.02 with 322.0 toughness and 1,131.5% elongation, was not chosen as best overall because its contact angle and stiffness were lower. Selecting on a single metric picks the wrong grade. Balance contact angle, toughness, stiffness, and cost against the actual service requirement.

Can this modification run on standard compounding equipment?

The laboratory work used an internal mixer, 10 minutes at 100 degrees Celsius followed by 20 minutes at 180 degrees Celsius, then compression molding at 180 degrees Celsius. Those temperatures are within normal PP processing range, so twin screw extrusion and injection molding should be feasible. Shear history and cooling rate differ, so expect to re-optimize the loading level.