Every mold shop has had the same bad day. Same resin, same tool, same press, and the parts still come out with sink marks, flash, silver streaks, or weld lines that wander around from shot to shot while the operator on the next machine runs the same job clean.

Most of that gap comes down to method. Around nine out of ten molding defects trace back to five places: material, mold, machine, process parameters, and part design. Once you can sort a defect into one of those five, troubleshooting stops being guesswork and starts being a checklist.

Below are the 13 defect families that show up most often on the floor, what causes each one, and the adjustments that clear them. It is written for process engineers, set-up technicians, and quality staff who need an answer before the next shot cycle rather than a textbook chapter.

The five places to look first

Run every defect through these five buckets before you touch a parameter. Most people jump straight to parameters because they are the easiest thing to change, and that is exactly why problems come back.

  1. Material. Moisture content, batch variation, regrind ratio, pellet size uniformity, contamination, thermal stability.
  2. Mold. Venting, cooling balance, gate and runner size, surface polish, parting-line fit, sliding core clearance.
  3. Machine. Clamp tonnage, check ring and screw wear, heater bands and thermocouples, hydraulic stability.
  4. Process parameters. Melt and mold temperature, injection speed and pressure, hold pressure and time, back pressure, screw recovery speed, cushion, cooling time.
  5. Part design. Wall thickness distribution, rib and boss geometry, sharp corners, abrupt transitions, draft angle.

A defect that improves after a parameter change and then reappears an hour later is usually a mold or machine fault wearing a process band-aid.

One habit matters more than any individual fix. Change one variable, then let the process settle for 10 to 20 shots before you judge the result. Molding is a thermal system with lag, and moving five things at once teaches you nothing.

1. Sink marks, shrinkage voids, and bubbles

Sink marks are surface depressions. Shrinkage voids are vacuum cavities inside thick sections. Bubbles are trapped moisture, air, or volatiles. All three come from volumetric shrinkage as the melt cools, and each one needs a different fix.

Sink marks show up where ribs, bosses, and thick sections meet the nominal wall, which is the last area to freeze and the first to pull in. Voids sit inside heavy walls where the skin has already solidified and the core has nothing left to draw from. Bubbles point at the material rather than at the packing stage.

Process adjustments:

  • Increase shot volume and injection pressure, and raise back pressure enough to homogenize the melt.
  • Extend injection time and cooling time so the gate has time to seal.
  • Raise injection speed where the flow length demands it.
  • An undersized gate freezes before packing finishes. Enlarge it.

Mold work:

  • Give thick walls, ribs, and bosses their own cooling circuits instead of relying on general cavity cooling.
  • Clean up the cold slug well so the frozen front stays out of the cavity.
  • A worn check ring lets hold pressure bleed back into the barrel. If pressure will not hold, pull the screw.

You can test the check ring without tearing the machine down. Run ten consecutive shots and compare the cushion on each one. Variation above 0.5 mm means the non-return valve is damaged. On very small parts with tiny shot volumes the test loses sensitivity, so read the pattern across many shots and combine it with how packing pressure behaves.

On the design side, keep rib thickness at 0.5 to 0.7 mm and thin the ribs further at locations far from the gate. Core out bosses with a crater design so material does not pile up locally.

Two tricks worth keeping. Sink marks caused by thin walls pulling inward sometimes clear when you add material locally and thicken the frozen layer at that spot. Rib networks that sink and stick in the cavity respond to vented ejector pins and rib ends cut to a ball profile.

2. Short shots

A short shot is a part that froze off before the cavity filled. It happens at the end of fill, never at the gate, which rules out half the theories people offer when a part comes out incomplete.

Common causes:

  • Melt temperature or mold temperature too low.
  • Injection pressure or shot volume too low, injection speed too slow.
  • Venting blocked or inadequate, so trapped gas stalls the flow front.
  • Runner or gate too small for the wall thickness and flow length.
  • Worn check ring or screw cutting effective shot delivery.

Fixes:

  • Raise barrel, nozzle, and mold temperature.
  • Increase injection pressure, shot volume, and injection speed.
  • Add or clean venting at the last areas to fill.
  • Inspect and repair the screw and non-return valve.
  • For ultra-thin parts, gas-assisted injection will push the flow front through when pressure alone cannot.

3. Flash and burrs

Flash is material squeezed out of the cavity into parting lines, slides, inserts, and ejector pin clearances. Either something let the melt go where it should not, or cavity pressure beat the clamp.

Machine causes:

  • Clamp force too low for the projected area and injection pressure.
  • Worn toggle linkage or cylinder seals, so clamp force drops under load.
  • Runaway temperature control. A failed thermocouple or heater band lets actual melt temperature exceed the setpoint and drops viscosity.

Mold causes:

  • Unbalanced loading across cavities, so one side opens slightly.
  • Excessive clearance on sliding cores and inserts.
  • Poor venting, where compressed gas inside the cavity forces the parting line open.

Process and material causes:

  • Resin flowability too high for the tool, or too much lubricant in the compound.
  • Pressure, speed, or temperature set too high. Use staged injection instead of one high-velocity fill.

Then there is the combination that makes people tear their hair out: short shot and flash on the same part. Look for uneven pellet size, a worn nozzle head or check ring letting melt flow back, an unstable cushion, or a failed gate cooling circuit. Check the non-return valve assembly first, since it accounts for most of these cases.

4. Burn marks and black specks

Burn marks are degraded, charred plastic carried into the cavity. Black specks are carbonized particles from material that decomposed in the barrel. Both mean the resin spent too long somewhere too hot.

Where to look:

  • Machine. Temperature control runaway, and worn screw or barrel surfaces where material hangs up and cooks. ABS and PVC crosslink and char especially fast at high temperature.
  • Mold. Vent grooves too shallow or blocked, runners and gates so small that shear heating overheats the melt, and excess mold release agent or oil contaminating the cavity.
  • Material. High moisture, foreign contamination, dirty regrind.
  • Process. Excessive injection pressure, back pressure, or screw speed all add shear heat. Purge and clean the barrel on a schedule, not when someone complains.

5. Weld lines

A weld line forms where two melt fronts meet and fail to fuse. The part looks acceptable and its strength at that line drops substantially, which is why weld lines cause field failures rather than scrap.

Mold actions:

  • Raise local mold temperature at the weld region.
  • Enlarge runners and cold slug wells so the fronts meet hotter.
  • Relocate gates to move the weld away from inserts, holes, or load-bearing areas.
  • Vent the convergence point fully. Trapped gas is often the reason the fronts never fuse.

Process actions:

  • Increase injection pressure.
  • Set injection speed deliberately. High speed brings the fronts together while they are still hot, low speed gives gas more time to escape. Choose based on whether the visible mark looks like a cold line or a gas burn.
  • Control barrel and nozzle temperature.
  • Cut back on silicone-based mold release, which contaminates the interface.
  • Raise back pressure moderately to homogenize the melt.

Design and material:

  • Avoid abrupt wall thinning near the meeting point.
  • Revisit insert placement.
  • Dry the material. Moisture flashes to gas exactly where the fronts meet.

6. Silver streaks

Silver streaks are the signature of moisture. Water in the resin flashes to steam during plasticizing and leaves silvery streaks radiating from the gate. If you see splay, dry the material before you do anything else.

Drying reference: dry at 10 to 15°C below the resin’s heat deflection temperature. For high-requirement PMMA parts, dry at 75 to 85°C for 3 to 6 hours.

Two other things produce the same look: excessive residence time in the barrel, which degrades the melt, and mixing incompatible resin types or grades.

Fixes: dry the resin thoroughly, lower melt temperature to prevent degradation, improve venting so volatiles escape, and reduce mold release agent.

7. Cracking and crazing

Cracking and crazing are residual internal stress becoming visible. The part can look fine coming out of the tool and crack hours later, or crack the moment it meets a solvent.

Causes:

  • Injection pressure and speed too high.
  • Poor gate design, especially gates that are too small or badly located.
  • Trapped gas.
  • Mold or melt temperature too low, freezing in orientation stress.
  • Abrupt wall thickness changes.
  • Abnormal ejection force, usually from under-polished or under-drafted cavities.
  • Chemical or solvent attack during downstream handling.

Mold fixes: enlarge and relocate the gate and runner, round off sharp corners, add venting ejector pins where gas traps, and preheat inserts.

Process fixes: tune injection and hold pressure and time, move melt and mold temperature in the right direction, reduce screw speed, and anneal finished parts to relieve stress.

One production rule pays for itself: never wipe parts with corrosive solvents. It is a common cause of delayed crazing that then gets blamed on the molding process.

8. Poor surface gloss and low clarity

Poor gloss usually means the melt froze before it could replicate the cavity surface. Low clarity in transparent parts usually means bubbles, silver streaks, or internal stress are scattering light.

Gloss: the main causes are poor cavity polish and premature melt freezing. Raise melt temperature, mold temperature, and injection pressure, optimize the gate and runner, and extend hold time and cooling time.

Clarity: silver streaks, bubbles, and residual stress all destroy transparency. Dry the material thoroughly, use staged melt temperature control with a moderately higher mold temperature, reduce injection speed while raising injection pressure, improve venting, and set back pressure and screw speed sensibly.

9. Flow marks, gas streaks, and gate ripples

Flow marks are wave patterns left by an unstable flow front. Gas streaks and gate ripples are dense ripples near the gate, caused by high-viscosity melt repeatedly freezing and re-melting as it enters the cavity.

Flow marks come from incomplete melting, mold temperature too low, unbalanced injection speed and pressure, an undersized gate, or a drastic thickness change. Raise melt temperature, mold temperature, and back pressure, rebalance speed and pressure, and revise the part geometry or gate location if the mark survives.

Gas streaks and gate ripples respond to higher nozzle and mold temperature, higher injection pressure and speed, larger gate and runner, a bigger cold slug well with stronger venting, and avoiding a design that is too thin at the gate.

10. Color variation, black streaks, specks, and delamination

Color defects come from thermal degradation, contamination, and poor dispersion. Delamination, where the surface peels in layers, comes from incompatible materials or a melt that never homogenized.

Color variation, black streaks, and specks: check for barrel overheating and degradation, carbon buildup from a worn screw and barrel, shear overheating from poor venting, and contamination from resin or regrind. Verify heater bands and thermocouples, service the screw and check-ring assembly, and control the regrind ratio.

Delamination: barrel or nozzle temperature too low and back pressure too low are the usual suspects, along with PVC injected too fast into a cold mold. Mixing different plastics or running contaminated resin is the most common cause of true layer separation.

If thick sections blister, lower mold temperature, extend cooling time, reduce processing temperature, increase hold pressure and time, and fix the wall thickness transition.

11. Nozzle drool and blockage, screw slip, sprue stringing

These are machine and process faults rather than part defects, and they stop production just as effectively.

Nozzle drool and blockage come from poor nozzle contact or insufficient clamp force, melt temperature too high, and injection pressure too high, plus blockage from cold plugs or foreign material. Lower the temperature, adjust injection pressure, service the nozzle, and clean out cold material.

Screw slip and plasticizing noise point to temperature too high or plasticizing temperature insufficient, and to feed throat bridging or freeze-off.

Safety warning: when clearing a feed throat blockage, put the machine in manual mode and use only a copper rod. Never use screwdrivers, steel bars, or other hard objects. Compressed gas and melt can blow back out of the feed opening and cause serious injury.

Sprue stringing means the melt temperature is too high. Apply a suck-back of 5 to 6 mm and lower nozzle temperature. Glass-filled PA66 has to be dried thoroughly, or the stringing returns no matter what you do to the temperature.

12. Masterbatch and coloring problems

Most color consistency problems are dispersion and compatibility problems.

Pigment streaking means the masterbatch is not dispersing, usually from a poor barrel temperature profile or insufficient back pressure. Raise the feed-zone temperature and increase back pressure. If that fails, check whether the masterbatch carrier resin matches the base polymer.

Parts cracking after masterbatch is added usually means the carrier’s additives or dispersants are incompatible with the base resin and are degrading its mechanical properties. Change the masterbatch grade.

Color drifting light and dark comes from metering inaccuracy, a mismatch between masterbatch and base resin in melt flow index or density, different heating conditions between machines, and the natural base-color variation you get between ABS batches.

Fading and poor gloss over time trace to insufficient dispersion, excessive titanium dioxide loading, or nozzle temperature and mold polish below standard.

13. Demolding difficulty, warpage, and dimensional instability

This is the family that most often sends a part back to design review instead of back to the press.

Demolding difficulty: insufficient ejection force, inadequate draft angle, mold temperature too high, rough runner or cavity surface, injection or hold or cooling time set too long, and insufficient internal lubricant.

Warpage: poor gate location and uneven ejection force, melt and mold temperature too high, excessive pressure with unbalanced hold and cooling time, abrupt wall thickness changes, and certain pigments that alter crystallization behavior.

Dimensional instability: fluctuating back pressure, temperature control, or hydraulics; unbalanced mold cooling circuits; resin batch variation; pellet size and moisture fluctuation; wear at the gate and runner.

Dimensional drift that appears gradually over a run is nearly always thermal. Check cooling circuit balance and barrel temperature stability before you touch the process.

A working order for troubleshooting

Run the defect through this sequence and most issues resolve in under an hour.

  1. Confirm the defect location and whether it repeats. Every shot means mold or design. Intermittent means machine wear or material variation.
  2. Check material first. Moisture and batch variation are cheap to rule out and cause an outsized share of defects.
  3. Verify machine condition. Cushion stability across ten shots tells you more about screw and check ring condition than any parameter readout.
  4. Adjust process parameters one at a time, letting the process stabilize between changes.
  5. Consider mold or design changes last, and write down what you did so the next shift does not repeat the work.

Keep a log

One line per event: part number, defect, what you changed, what happened next. After a quarter of entries, the same sink mark on the same tool stops arriving as a fresh problem, because the fix is already in the file and the second occurrence takes minutes instead of a shift.