Long chain nylon grades are polyamides carrying ten or more carbons between amide groups, which is why they hold a small fraction of the water that PA66 does. Four members do nearly all the commercial work: PA12, PA11, PA610 and PA1010. Each one gives up stiffness and heat resistance in exchange for dimensional stability, toughness in the cold and resistance to chemicals, and each one sells for two to three times the price of a short chain nylon.
Degrees Celsius covers temperature throughout, Charpy impact is notched and given in kJ/m2, stress and modulus in MPa, density in g/cm3, and price in RMB per tonne.
What counts as a long chain nylon grade
Every polyamide alternates amide groups with runs of methylene, and counting the carbons in those runs is what separates this family from PA6 and PA66. The stricter definition asks for at least 10 methylene groups between adjacent amide groups. Suppliers and engineers generally use a looser one instead: count the carbons in the repeat unit, and call anything at 10 or above long chain. Long chain polyamide is the formal label for exactly the same materials.
Those two definitions do not agree, and the disagreement is worth knowing because people quote whichever one helps their case. PA11 and PA12 clear both comfortably. PA610 fails the strict test, since its repeat unit holds 16 carbons wrapped around 2 amide groups, which comes to 8 carbons per grip. Nobody argues about whether PA610 belongs, though. Long chain is a commercial grouping, not a clean threshold.
The grouping covers PA11, PA12, PA610, PA612, PA1010, PA1012 and PA1212. Transparent nylon belongs to the wider clan and draws on PA12 chemistry, although most transparent grades are semi-aromatic rather than true long chain aliphatic nylons.
Grade names tell you what the polymer was built from. A single number means one monomer brought all its carbons along, as in PA6, PA11 and PA12. Two numbers mean a diamine met a diacid, and the pair of numbers gives the carbon count on each side.
Table 1. What the grade numbers mean for each long chain nylon member
| Grade | First number | Second number | Repeat unit carbons | Amide groups per repeat unit | Carbons per amide group |
| PA6 | 6 carbons in the caprolactam monomer | none, single monomer route | 6 | 1 | 6 |
| PA66 | diamine with 6 carbons | diacid with 6 carbons | 12 | 2 | 6 |
| PA610 | diamine with 6 carbons | diacid with 10 carbons | 16 | 2 | 8 |
| PA612 | diamine with 6 carbons | diacid with 12 carbons | 18 | 2 | 9 |
| PA1010 | diamine with 10 carbons | diacid with 10 carbons | 20 | 2 | 10 |
| PA1012 | diamine with 10 carbons | diacid with 12 carbons | 22 | 2 | 11 |
| PA11 | 11 carbons in the amino acid monomer | none, single monomer route | 11 | 1 | 11 |
| PA12 | 12 carbons in the laurolactam monomer | none, single monomer route | 12 | 1 | 12 |
| PA1212 | diamine with 12 carbons | diacid with 12 carbons | 24 | 2 | 12 |
Divide repeat unit carbons by amide count and you get carbons per amide group, which is how PA1212 arrives at the same 12 as PA12. The family melts between 178 and 220 degrees Celsius, a notch under PA6 and PA66, and every member is a semi-crystalline thermoplastic shipped as translucent cylindrical pellets in milky white to faintly yellow tones. Castor oil gives PA11 a slight natural tint, while PA12 comes out whiter.
One distinction needs clearing up before you ask a supplier for anything. Long chain describes the carbon run sitting between amide groups, and the monomer decides it. Molecular weight is a separate dial, turned by degree of polymerization. Better melt strength or higher viscosity means asking for viscosity or molecular weight. Asking for a longer chain gets you something drier, not something tougher.
Why amide density drives every long chain nylon property
Two structural pieces do all the work here, and their ratio explains everything else in this article.
Amide groups are the grips. Each carries a polar CO-NH pair, forms hydrogen bonds with its neighbors, and gives nylon its stiffness, strength and heat resistance. Those same sites are how water gets in. Water molecules are polar and go looking for exactly those places.
Methylene runs are the soft parts. No polarity, no hydrogen bonds, nothing to absorb, and enough freedom for the chain to bend.
Stretch out the methylene and the grips get diluted. The chain of consequences is short enough to keep in your head: a longer carbon run lowers amide density, and lower amide density lowers water absorption, density, melting point and internal stress while raising flexibility and dimensional stability. Stiffness and heat resistance go down with them.
PA66 against PA12 makes the point better than any diagram. Both repeat units have 12 carbons, which makes them look like relatives. Their water absorption differs by 5 to 10 times because PA66 packs 2 amide groups into that repeat unit, averaging 6 carbons per grip, while PA12 carries 1, at 12 carbons per grip. Repeat unit carbon count is never the number to read on its own. Carbons per amide group is.
That one number also explains why this family cannot simply take over from PA6 and PA66. Each end of the nylon range answers a different question. Short chain nylon wins when stiffness per unit of cost is the priority and humidity drift is tolerable. Longer chain members win when a part has to hold tolerance through humidity swings, survive cold, or spend ten years in fuel or glycol.
Long chain nylon grades compared across structure and properties
Keep the table below open while shortlisting. It sets the four workhorse grades beside PA6 and PA66 with typical melting point, density and equilibrium water absorption. Long chain nylon water absorption and long chain nylon melting point are the same amide density read off in different units, and long chain nylon price lines up with both.
Table 2. Structure and typical physical properties of long chain nylon grades against PA6 and PA66
| Grade | Carbons per amide group | Melting point | Density | Equilibrium water absorption |
| PA6 | 6 | 215 to 225 | 1.13 | 2.5 to 3.0 percent |
| PA66 | 6 | 255 to 265 | 1.14 | 2.5 percent |
| PA11 | 11 | 186 | 1.04 | 0.30 percent |
| PA12 | 12 | 178 | 1.01 | 0.25 percent |
| PA610 | 8 | 220 | 1.07 | 0.35 percent |
| PA612 | 9 | 212 | 1.06 | 0.25 percent |
| PA1010 | 10 | 200 | 1.05 | 0.39 percent |
| PA1012 | 11 | 192 | 1.04 | 0.30 percent |
The whole commercial argument sits in the water absorption column. Everything from PA610 upward sits below 0.4 percent while PA6 and PA66 sit between 2.5 and 3.0 percent. That is a 6 to 10 fold gap in how much water the polymer holds, and the same multiple applies to how far the part moves and how much its electrical behavior drifts.
Cost comes through in the melting point column. PA610 reaches 220 degrees Celsius, the highest figure in the table, because its 16 carbon repeat unit still carries 2 amide groups. PA12 stops at 178 degrees Celsius, a full 80 degrees Celsius below PA66, which is why it has no place near a hot engine bay.
Remember that carbons per amide group is an average, and averages hide shape. AABB types such as PA610 alternate a 6 carbon diamine segment with a 10 carbon diacid segment, so local environments vary even though the mean reads 8. AB types such as PA11 and PA12 run one uniform segment the whole way through.
The four workhorse long chain nylon grades and how they divide the work
Four grades carry most of the volume. Each has a route, an origin and a temperament, and choosing between them mostly comes down to which compromise you can live with.
Table 3. The four workhorse long chain nylon grades side by side
| Grade | Polymerization route | Monomer origin | Bio-based carbon | What it is good at |
| PA12 | ring-opening of laurolactam | petrochemical route | 0 percent | lowest density at 1.01, lowest absorption, widest processing window, largest global volume |
| PA11 | polycondensation of 11-aminoundecanoic acid | castor oil | 100 percent | melting point 186, better elasticity and impact than PA12, the long standing air brake tube standard |
| PA610 | diamine plus sebacic acid | sebacic acid from castor oil | 56 to 64 percent | melting point 220, clearly stiffer than PA12, roughly half the PA12 price |
| PA1010 | diamine plus sebacic acid | both monomers available from castor oil | 100 percent | melting point 200, good light transmission, strongest local industrial base |
PA12 is the default answer. Its density of 1.01 is the lowest anywhere in the nylon family, 8 to 12 percent lighter than PA66 at equal volume, its water absorption is the lowest, and its melt viscosity behavior is forgiving across injection molding, pipe extrusion, blow molding and powder bed sintering without needing a separate grade family for each.
PA11 is the specialist choice. It costs more, comes from castor oil, carries 100 percent bio-based carbon, and recovers from deformation better. That combination is why it became the standard material for air brake tubing, where a tube takes repeated pressure pulses at low temperature for years.
PA610 is what you reach for when you want most of the humidity advantage without paying PA12 prices. Its sebacic acid half originates in castor oil, it holds a melting point of 220 degrees Celsius, 40 degrees above PA12, and it is measurably stiffer.
PA1010 offers the widest local supply base available today and a path to 100 percent bio-based carbon with properties sitting mid range. It also transmits light better than the rest, which puts it close to transparent work. Grades built on those monomers also sell as bio-based nylon, and with the route starting in castor oil they turn up in supplier lists as castor oil nylon too.
Why PA11 melts higher than PA12 despite having fewer carbons
This is the result that trips people up. PA11 runs 11 carbons per amide group against 12 for PA12, and the structural rule says more carbons means a lower melting point. PA11 should melt lower. It melts at 186 degrees Celsius against 178 for PA12, and it returns to shape better too.
Odd-even packing explains it. PA11 is an odd carbon AB nylon, its chains stack in the crystal differently than even carbon PA12 does, and that arrangement gives it the higher melting point and better elastic recovery. PA12 spends its structural regularity on more perfect crystallization, and that is precisely what buys dimensional stability and barrier performance against vapor.
Worth carrying into the next design meeting: pick PA11 when the part needs spring and impact, pick PA12 when it needs to hold its shape and keep vapor out. Both statements come down to how chains pack, not to how many carbons sit between grips, and neither grade is stronger in any general sense.
What an unfilled PA12 datasheet actually says
Family typical values hide the detail a designer needs. The table below takes one unfilled general purpose PA12 of high viscosity, described in its own documents as aimed at termite resistant cable, functional cable and pipe fittings, and reproduces the published datasheet column.
Table 4. Typical properties of an unfilled high viscosity PA12 general purpose grade
| Property | Test standard | Unit | Typical value | What it means in practice |
| Density | ISO 1183 | g/cm3 | 1.00 | about 12 percent lighter than PA66, so equal volume costs less material |
| Equilibrium water absorption at 23 degrees Celsius and 50 percent RH | ISO 62 | percent | 0.5 | PA66 reads 2.5 percent on the same basis, five times higher |
| Tensile modulus at 23 degrees Celsius | ISO 527 at 1 mm/min | MPa | 1250 | about 40 percent of PA66 stiffness, wins on toughness instead |
| Tensile yield stress at 23 degrees Celsius | ISO 527 at 50 mm/min | MPa | 41 | about half PA66, so not for load bearing structure |
| Nominal strain at break | ISO 527 at 50 mm/min | percent | over 150 | absorbs assembly strain and impact without failing |
| Charpy notched impact at 23 degrees Celsius | ISO 179 | kJ/m2 | 15 | good at room temperature |
| Charpy notched impact at minus 30 degrees Celsius | ISO 179 | kJ/m2 | 6 | drops sharply, so cold parts need their own check |
| Melting point | ISO 11357 | degrees Celsius | 177 | about 80 degrees Celsius below PA66 |
| Deflection temperature under load at 0.45 MPa | ISO 75 | degrees Celsius | 115 | workable at low load, falls clearly at 1.8 MPa |
| Documented target uses | termite resistant cable, functional cable, pipe fittings | described as high viscosity, resistant to light and heat ageing, excellent permeation resistance |
Molding shrinkage and flexural modulus are not published for this grade, and neither figure is invented here. One warning belongs beside the table: a plasticized flexible pipe grade from the same series lists modulus at 520 MPa and notched impact at 105 kJ/m2 at 23 degrees Celsius. Those describe different material, and they have no business in a calculation built on the table above.
Two lines settle most decisions. Modulus reads 1250 MPa where PA66 sits near 3000 MPa, and water absorption reads 0.5 percent where PA66 reads 2.5 percent. Stiffness is being traded for dimensional stability, heat resistance for low temperature behavior. In pipe, sheathing, lining or small precision parts that trade pays off. In a bracket designed around PA66, it does not.
Where long chain nylon grades earn their price
Applications bunch up tightly. Longer chain nylons go into parts that sit against oil, water or cold for years and still have to hold their shape, and nowhere else, because PA6 or PA66 handles everything else for a fraction of the cost. Automotive takes 45 to 50 percent of the whole market on its own.
Table 5. Where each application uses long chain nylon grades and why
| Field | Typical parts | Why this material rather than PA66 |
| Automotive tubing | fuel line, hydraulic line, vacuum line, air brake tube, electric vehicle cooling line | low extractables, fuel resistance, permeation resistance, flexibility |
| Automotive braking | air brake tube, where PA11 is the long standing standard | hydraulic fluid resistance, low temperature behavior, fatigue pulse life |
| Wire and cable | submarine cable sheathing, termite resistant cable, optical fiber sheathing | seawater resistance, abrasion resistance, flexibility, permeation resistance |
| 3D printing | PA12 powder for laser sintering, about 60 percent of polymer powder consumed in 3D printing | low melting point, wide sintering window, low water absorption so the powder stores well |
| Transparent parts | electronic cigarette liquid tanks, high end spectacle frames, transparent medical fluid containers | light transmission over 85 percent, chemical resistance, sterilizable |
| Precision mechanics | precision gears, bearing cages, quick connectors, bushings | low absorption holds tolerance, glass or carbon fiber can raise stiffness |
| Powder coating and medical | fluidized bed dipping, electrostatic spray, catheters and device parts | abrasion and corrosion resistance, biocompatibility, radiolucent |
Two entries need more space.
Battery cooling circuits come first. Such a circuit needs low water absorption, glycol resistance, dimensional stability and freedom from long term embrittlement, all at the same time. PA12 is the mainstream international answer, and PA1012 along with several other long chain grades are going into the same duty. For locally made PA12 this is the biggest pool of new demand anywhere.
Transparent nylon comes second, sharing chemistry with PA12 while mostly belonging to the semi-aromatic branch rather than the long chain aliphatic one, so it sits in the wider family. More than 85 percent of visible light gets through, and it resists stress cracking better than polycarbonate, which lands it in tanks for e-liquids, eyewear and medical devices. Local grades cover roughly 20 percent of that segment, and the high end still comes from overseas.
Choosing between PA12 PA610 and PA1010 without overpaying
Most long chain nylon projects die at the quote, and price is the reason. PA11 and PA12 sit between RMB 100,000 and 140,000 per tonne, imported PA11 can hit RMB 150,000 to 200,000, and short chain nylon costs several times less. PA610 and PA1010 come in at RMB 40,000 to 60,000 per tonne. If PA610 holds the tolerance and survives the fluid, buying PA12 means paying for headroom nobody will use. Two comparisons come up more than any other. PA11 vs PA12 turns on how chains pack, and PA12 vs PA66 turns on whether the part needs dimensional stability enough to justify the price.
Table 6. Shortlisting long chain nylon grades by duty and budget
| If the part needs | Start here | Do not start here | Why |
| Lowest water absorption and best dimensional stability | PA12 | PA6 or PA66 | PA11 and PA12 sit under 0.35 percent where short chain nylon sits at 2.5 to 3.0 percent |
| High spring back and impact, especially in braking | PA11 | PA12 | odd carbon packing gives PA11 better elastic recovery |
| Stiffness above the PA12 line with most of its humidity advantage | PA610 | PA12 | PA610 melts at 220 and costs about half as much |
| 100 percent bio-based carbon with mid range properties | PA1010 or PA11 | PA12 | PA12 has no bio-based route at present |
| Melting point above 210 with creep resistance | PA610 | PA12 | highest melting point in the family at 220 |
| Lowest cost while staying below 0.4 percent absorption | PA610 or PA1012 | PA11 or PA12 | two to three times cheaper |
| Laser sintering powder stability | PA12 | PA11 | wide sintering window and low absorption keep the powder usable between builds |
Three numbers decide whether stepping down works. Check continuous service temperature against the 90 to 120 degrees Celsius band the family generally supports. Check impact at cold, not at room temperature. Check whether the chemicals involved justify low amide density at all. If all three pass on PA610, defending PA11 or PA12 gets difficult.
Representative long chain nylon grades by tier
The tier structure and the figures that separate grades survive here; the commercial names do not. Every row corresponds to a grade with published technical data.
Table 7. Representative grades by tier, with commercial names removed
| Tier | Representative source | Key published figures | Where it runs |
| PA12 general purpose | one fully integrated domestic producer, unfilled high viscosity | density 1.00, water absorption 0.5 percent, light and heat ageing resistance, excellent permeation resistance | termite resistant cable, functional cable, pipe fittings |
| PA12 flexible pipe | same domestic producer, plasticized | modulus 520 MPa, notched impact 105 kJ/m2 at 23 degrees Celsius | fuel line, hydraulic line, cable sheathing |
| PA12 with 30 percent glass fiber | same domestic producer | modulus 6800 MPa, deflection temperature 165 at 1.8 MPa | electrical parts, quick connectors |
| PA12 with 40 percent carbon fiber | same domestic producer | modulus 23000 MPa, deflection temperature 170 at 1.8 MPa | lightweight structural parts, sports equipment |
| PA12 partly bio-based | an overseas producer | 30 percent bio-based carbon, heat and UV stable, low absorption, scratch resistant | sports and consumer goods injection molding |
| PA12 long carbon fiber | an overseas compounder | 40 percent carbon fiber, tensile 260 to 290 MPa, flexural modulus 21000 to 23000 MPa | high stiffness impact resistant parts |
| PA11 pipe extrusion | the sole overseas producer | castor oil based, 100 percent bio-based, low oligomer, melting point 182, density 1.00 | pipe extrusion |
| PA11 fuel line | the sole overseas producer | black bio-based pellets, melting point 186, impact resistant, low absorption | automotive fuel lines and industrial hose |
| PA610 | one Swiss compounder | bio-based high viscosity, modulus 2200 MPa, melting point 223, shrinkage 1.3 to 1.4 percent | injection molding and extruded film |
| PA610 soft injection | one European producer | density 1024 kg/m3, notched impact 18 kJ/m2 at minus 30 degrees Celsius | ski boots, sports shoes |
| PA610 general purpose | one European compounder | unfilled, bio-based carbon 56 percent, modulus 2300 MPa, melting point 220 | low absorption chemical resistant parts |
| PA1010 | one overseas producer | 100 percent bio-based carbon, density 1.04, melting point 200, modulus 1700 MPa | spectacle frames and monofilament |
| PA1010 with 30 percent glass fiber | one Swiss compounder | modulus 11000 MPa, melting point 200, laser direct structuring grade | automotive electronics and connectors |
Batch variation and differing test standards move all of these figures. Ask for the current datasheet before anything reaches a drawing.
Processing long chain nylon grades without the usual defects
Low water absorption is not permission to skip drying, and this is where most first runs go wrong. Half a percent of moisture hydrolyzes at 250 degrees Celsius, and it shows up as silver streaking and gas marks on parts that were supposed to be easy.
Table 8. Processing window for PA12 and PA11
| Item | Setting | Note |
| Drying | dehumidifying dryer at 80 to 90 degrees Celsius for 2 to 4 hours | target moisture before processing at most 0.05 to 0.1 percent |
| Melt temperature, unfilled PA12 | 220 to 260 degrees Celsius | low melt viscosity, so watch for nozzle drool |
| Melt temperature, glass or carbon fiber reinforced | 240 to 280 degrees Celsius | special grades go up to 300 |
| Melt temperature, PA11 pipe extrusion | 230 to 270 degrees Celsius | |
| Mold temperature, general work | 40 to 60 degrees Celsius | do not copy PA6 and PA66 settings here |
| Mold temperature, thin wall high gloss or precision | 60 to 80 degrees Celsius | too cold leaves high internal stress and a dull surface |
| Pipe extrusion | 210 to 260 degrees Celsius | |
| 3D printing filament cooling water | above 40 degrees Celsius | avoids quench warpage |
| Screw hardware | watch non-return valve clearance | low viscosity melt leaks back through worn clearances |
| Fiber grades | control shear, use wear resistant mold steel | |
| Post treatment | anneal or condition pipe parts | stabilizes dimensions |
| Plasticized grades | avoid long high temperature exposure | keeps plasticizer from migrating out |
Say this one out loud in the tool room: running PA12 at the 80 to 120 degrees Celsius mold temperatures that PA6 and PA66 prefer will over crystallize it, stretch the cycle, and leave shrinkage less predictable rather than more.
Six ways long chain nylon grades get mis-specified
These failures show up in parts rather than datasheets, so read them before cutting steel.
Using PA12 as a straight substitute for PA66. Its modulus is 1250 MPa, melting point 177 degrees Celsius, and deflection temperature 115 degrees Celsius at 0.45 MPa. Dropped into a heat resistant structural part designed around PA66, it deforms.
Deciding the material absorbs too little to need drying. What counts is what happens at processing temperature, and 0.5 percent hydrolyzes.
Borrowing short chain mold temperatures. Warmer does not mean safer for PA12, and past 80 degrees Celsius you are buying crystallization trouble.
Designing cold service from room temperature data. Notched impact drops from 15 kJ/m2 at 23 degrees Celsius to 6 kJ/m2 at minus 30 degrees Celsius on the reference grade, and plasticized flexible grades drop further.
Bonding, printing or hot stamping with no surface treatment. Surface energy sits low, so direct bonding fails and plasma or flame treatment or a primer comes first.
Paying for capability nobody uses. PA11 and PA12 run two to three times the cost of PA610 and PA1010, and a lot of applications sit comfortably in the cheaper band.
How supply of long chain nylon grades is changing
Four overseas producers held PA12 entirely for most of its history. That ended after a domestic producer launched its project in 2012 and brought an integrated 40,000 tonne per year plant on stream in October 2022, becoming the first in Asia and the second worldwide to run the full route from monomer through polymer. Buying prices inside the country fell by about 20 to 30 percent, and local material now covers roughly 40 percent of demand.
PA11 is a different situation, and it remains the hardest bottleneck anywhere on the long chain nylon chain. One industrial producer serves the world, local capacity is zero, and the route to aminoundecanoic acid, its monomer, is proprietary. Those facts explain the RMB 150,000 to 200,000 per tonne price tag, and they mean anyone writing PA11 into a specification should plan around a single source.
High end transparent nylon sits in much the same position, dependent on imports, with local material covering about 20 percent of the segment.
Anyone buying PA12 faces a genuinely better market than five years ago, mostly because integration moved upstream. Anyone buying PA11 faces the same market they always did, and no amount of grade shopping changes that.
Limitations
Everything here is typical value, not purchase specification. Grade variation, batch variation and differing test standards move every number in these tables, and the only defensible basis for a drawing is the manufacturer datasheet current on the day you order.
Two different conventions sit behind the water absorption figures. Family typical values in Table 2 put PA12 at 0.25 percent, the reference datasheet column in Table 4 puts it at 0.5 percent at 23 degrees Celsius and 50 percent RH, and summary references quote 0.25 to 0.5 percent. That spread reflects how it was measured, and it is reported rather than reconciled by guesswork.
Long chain itself is a soft category. The strict methylene test excludes PA610, which the industry counts without hesitation, so any claim about membership depends on which definition is in play.
The datasheet column carried in Table 4 publishes neither molding shrinkage nor flexural modulus, so those gaps stay empty instead of being filled from another grade. The figure for PA1212 comes from its monomer pair by arithmetic, not from measurement.
Supply and price statements reflect what the source material described. Both move quickly, above all for PA11, whose price follows a single producer.
Bottom line
What long chain nylon grades buy is threefold: stability against humidity, toughness at low temperature, and chemical resistance that lasts ten years in fuel or glycol. Payment comes as stiffness, heat resistance and price at roughly two to three times PA6 or PA66. Start at PA610 unless the duty genuinely needs what only PA11 or PA12 delivers, check cold impact at the real service temperature, and dry it even though it hardly takes up water.
FAQ
What is long chain nylon
Long chain nylon is a group of polyamides whose repeat units carry ten or more carbons, leaving ten or more carbons between neighboring amide groups. That spacing dilutes the polar amide sites, so the material absorbs far less water than PA6 or PA66, sits at lower density, melts lower, stays flexible in the cold and holds its dimensions through humidity swings.
How is long chain nylon different from PA6 and PA66
The difference is amide density. PA6 and PA66 average 6 carbons per amide group, while long chain nylon grades run from 8 to 12. Fewer amide sites mean water absorption drops from 2.5 to 3.0 percent down to 0.25 to 0.4 percent, while tensile modulus drops from roughly 3000 MPa to around 1250 MPa on unfilled grades.
Why does long chain nylon absorb so little water
Water enters nylon by bonding to polar amide groups. A long chain nylon puts more non polar methylene between those groups, so there are fewer sites per unit mass for water to reach. PA12 has one amide group per 12 carbons, PA66 has one per 6 carbons on average, and the two differ in water absorption by 5 to 10 times.
Which long chain nylon grade absorbs the least water
PA12 absorbs the least, at 0.25 percent typical, followed by PA612 at 0.25 percent and PA11 at 0.30 percent. PA610 sits at 0.35 percent and PA1010 at 0.39 percent. All sit far below the 2.5 to 3.0 percent typical of PA6 and PA66. Check the test basis, since some datasheets quote 0.5 percent for PA12 at 50 percent RH.
What is the melting point of long chain nylon grades
The family spans 178 to 220 degrees Celsius. PA12 melts lowest at 178 degrees Celsius, PA11 reaches 186, PA1010 reaches 200, PA1012 reaches 192, and PA610 is highest at 220 degrees Celsius. PA66 for comparison melts between 255 and 265 degrees Celsius, roughly 80 degrees Celsius above PA12.
Is PA12 strong enough to replace PA66 in structural parts
Not in unfilled form. A general purpose unfilled PA12 lists tensile yield stress of 41 MPa and tensile modulus of 1250 MPa, around half and around 40 percent of typical PA66 figures. Reinforced grades change the picture, since 30 percent glass fiber raises modulus to around 6800 MPa and 40 percent carbon fiber to around 23000 MPa.
Which long chain nylon grade should I use for automotive air brake tubing
PA11 is the traditional standard for air brake tubing because it combines hydraulic fluid resistance with low temperature toughness and long fatigue pulse life, and its odd carbon crystal structure gives better elastic recovery than PA12. PA12 is used widely for other automotive tubing such as fuel and vacuum lines where those demands are lower.
How do PA11 and PA12 compare
PA11 comes from castor oil with 100 percent bio-based carbon and melts at 186 degrees Celsius, higher than PA12 despite having fewer carbons between amides, because its odd carbon structure packs differently. PA12 melts at 178 degrees Celsius, has lower density at 1.01 against 1.04, offers better dimensional stability and gas barrier, and costs less. Pick PA11 for spring and impact, PA12 for stability.
Why is PA11 more expensive than PA12
PA11 relies on a single monomer, aminoundecanoic acid, whose synthesis route is proprietary to one industrial producer worldwide, and there is no alternative supply. Global capacity sits with one company, domestic capacity is zero, and prices reach RMB 150,000 to 200,000 per tonne against RMB 100,000 to 140,000 for PA12.
Do long chain nylon grades need drying before processing
Yes. Low absorption does not remove the need, because 0.5 percent moisture hydrolyzes at 250 degrees Celsius and produces silver streaking and gas marks. Dry PA12 and PA11 in a dehumidifying dryer at 80 to 90 degrees Celsius for 2 to 4 hours and get moisture below 0.05 to 0.1 percent. Transparent grades and extruded tube are more sensitive still.
Is long chain nylon suitable for 3D printing
PA12 is the dominant polymer powder for laser sintering, taking about 60 percent of polymer powder volume in 3D printing. It sinters well because the melting point is low and the sintering window is wide, and it stores well because low water absorption means the powder does not pick up moisture between builds.
When is PA610 the better choice over PA12
Choose PA610 when the part needs low water absorption plus more stiffness and higher heat resistance than PA12 can give, and when cost matters. PA610 melts at 220 degrees Celsius against 178 for PA12, costs roughly half as much, still holds water absorption near 0.35 percent, and carries 56 to 64 percent bio-based carbon from its sebacic acid half.