Melt flow rate is not a fixed material property. It is the result of one test run at a specified temperature, under a specified load, over ten minutes. Change any condition and the number changes. So a grade rated 19 and another rated 35 may not come from the same measuring stick at all.
Why one MFR number is not enough
Melt flow rate (MFR), also written MVR or MI, measures how much molten plastic a small die pushes out in ten minutes. You load the material into a heated cylinder, place a weighted piston on top, and collect what comes out the bottom. Three variables act together to set the result: temperature, load weight, and the ten-minute window. A data sheet showing only “MFR 20” has told you half the story.
Temperature and load both move the number. A hotter melt flows more easily. A heavier weight pushes harder. Together they can swing the result by a wide margin. So the number is meaningful only when you know the conditions that produced it.
MI stands for melt flow index and MVR stands for melt volume rate. Melt flow rate testing follows ISO 1133 and ASTM D1238.
Melt flow rate across six grades: six test conditions
Here is how six real grades appear on data sheets, with the conditions printed beside each value:
| Material | Grade | Table value (as printed) | Test condition |
| ABS | PA-757 | 19 ml/10min | 220 C x 10 kg |
| PP | JM-370 | 35 g/10min | 230 C x 2.16 kg |
| PC | PC-110 | 10 ml/10min | 300 C x 1.2 kg |
| GPPS | PG-33 | 8.0 cm3/10min | 200 C x 5 kg |
| PMMA | IF850 | 13 g/10min | 230 C x 3.8 kg |
| PBT | B6550 | MVR 9 cm3/10min | 250 C x 2.16 kg |
| HDPE | MF6000 | 0.4 g/10min | ASTM D1238 only; no temperature or load |
The spread is wide. Temperature runs from 200 C to 300 C, a hundred-degree gap. Load runs from 1.2 kg to 10 kg, more than eight times apart. Two rows carry extra traps:
- GPPS grade PG-33 is labeled “flow coefficient,” not MFR. It is the same quantity under a different name, easy to copy into a file as if it were another physical property.
- HDPE grade MF6000 cites only ASTM D1238 with no temperature or load. That standard lists several condition sets, so this number can only be compared within the same grade and batch, never across sources.
Melt flow rate is not a flow rating across materials
A higher MFR number does not mean better flow unless you are comparing the same material under the same conditions.
Take GPPS grade PG-33 (flow coefficient 8.0) versus ABS grade PA-757 (MFR 19). Numerically, 19 is more than double 8, so ABS looks like the easier-flowing material. In reality the opposite is true. Polystyrene flows more easily than ABS, which contains a rubber phase that makes it more viscous. The ABS number is inflated because its test used 10 kg of load at 220 C, while the GPPS test used only 5 kg at 200 C. Higher pressure plus higher temperature pushes the number up. You are comparing conditions, not materials.
That is the core rule: comparing MFR across material types is almost meaningless. Every material family has its own test tier. High-melting, viscous resins such as PC and PBT are tested at high temperature with light load. PP and PE use the light 2.16 kg tier. ABS pairs high temperature with heavy load. These tiers follow industry convention, which is exactly why cross-material numbers never sit on the same ruler. Melt flow rate temperature load settings are not interchangeable across materials.
MFR and MVR: weighed versus measured
MFR and MVR look like two unit systems, but they are two different quantities.
MFR is mass flow rate: what comes out is weighed, reported in g/10min. MVR is volume flow rate: what comes out is measured by volume, reported in cm3/10min. The ml/10min still seen on some sheets equals cm3/10min. It is not a third quantity.
One is weighed, the other is measured. They look convertible, but converting volume to mass requires melt density, and melt density changes with temperature. You cannot borrow someone else’s density and plug it in.
PBT grade B6550 shows the point: its sheet reports MVR 9 cm3/10min at 250 C x 2.16 kg and gives no MFR. The manufacturer simply reports by volume. Do not place an MVR figure next to an MFR figure and treat them as comparable.
MFR and molecular weight: one inverse chain
A high MFR means the melt flows fast under the same conditions. Fast flow means short molecular chains, low molecular weight, and few entanglements between chains. These three statements form one causal chain, not three separate phenomena.
Think of molecular chains as noodles. Short noodles slide past each other easily. Long noodles tangle and resist flow. So when you read an MFR number, you are seeing one side of molecular weight. Molecular weight melt flow runs in one direction: high MFR means low molecular weight.
High MFR buys easy mold filling and lower energy use. The other side of the trade is performance. Short chains and few entanglements mean the material absorbs impact less well. On a data sheet, this shows up as lower impact strength and lower elongation at break. The same grade also has lower melt strength, so in extrusion, blow molding, or foaming the melt can break or collapse. Resistance to environmental stress cracking drops too. A part under stress, sitting in oil or detergent, turns white and cracks more easily.
So “high MFR means easier processing” is only half true. Easy filling is real; the price is toughness and impact resistance. Impact strength MFR trades off against flow: high MFR grades lose impact strength. Processes such as injection molding and extrusion need adequate melt strength.
One material family, three grades
The same inverse line holds inside one material family. Take three impact-resistant copolymer PP grades from one producer:
| Grade | MFR | Typical use | Impact rating |
| 3015 | 2.0 | Paint cans, sports equipment, luggage | High impact |
| 3080 | 9 | Auto parts, electrical parts, office furniture | Medium impact |
| 3204 | 30 | Washing machine tubs, toolboxes, thin-walled parts | Medium impact |
The three numbers, from 2 to 30, say the same thing: MFR is not good or bad, only suitable or not. Within one material, the highest MFR and the highest impact almost never fall on the same grade. High MFR equals low molecular weight. Read the number together with what it gives up.
How to use it: three rules
- Compare only numbers from the same material, same standard, same temperature, same load. Miss one condition and it is not a comparison; it is only a reference.
- When changing material, align conditions first, then compare values. If the other side’s conditions do not match, ask for data under the same conditions, or run a trial yourself. Gambling a whole batch’s processability to save one test step is not worth it.
- Do not judge processability by MFR alone. Also look at melt strength, the width of the processing window, and the ratio of MFR values at different loads, which reflects molecular weight distribution breadth.
When you quote a number, the same rule applies: compare MFR only at the same material and same conditions. If a customer says “I saw 30 somewhere,” do not rush to explain high or low. Ask first: at what temperature, under what load, was that 30 measured? Get the order wrong and the conclusion is wrong.
MFR is not the personality of a material. It is one measurement under one set of conditions. Change the conditions, the action changes, the number changes. Ask about conditions first, then talk about size.
Limitations
Every MFR figure in this article comes from the condition printed beside it on a data sheet. A number tested at 220 C x 10 kg is not the same quantity as one tested at 230 C x 2.16 kg. This article does not provide material selection advice. Confirm values against the latest supplier data sheet and actual production conditions before use.
Bottom line
An MFR number is only half a sentence until you know the temperature, the load, and the ten-minute window. Never compare MFR across materials or across conditions. Compare only same material, same standard, same temperature, same load. And remember: higher MFR means easier flow but lower impact strength. Choose the grade that fits the part, not the biggest number. This article covers plastic melt flow rate and how to read the melt flow rate data sheet. Always check the material data sheet condition before quoting a number. Compare only same material same conditions: same standard, same temperature, same load.
FAQ
What is melt flow rate (MFR)?
It is the mass or volume of molten plastic extruded through a small die in ten minutes under a specified temperature and load. It is the result of one test under defined conditions, not an inherent property of the material.
Why can’t I compare MFR numbers across different plastics?
Because each material family is tested under its own conditions; different temperatures and loads apply. A high-melting resin such as PC may be tested at 300 C with 1.2 kg, while PP is tested at 230 C with 2.16 kg. The number reflects conditions as much as the material, so cross-material comparison is nearly meaningless.
What is the difference between MFR and MVR?
MFR is mass flow rate: the extruded material is weighed, reported in g/10min. MVR is volume flow rate: the extruded material is measured by volume, reported in cm3/10min. They are different quantities and converting between them requires melt density, which changes with temperature.
Does a higher MFR mean better flow?
Only when comparing the same material under the same conditions. Across materials, a higher number can come from a heavier load or higher temperature rather than easier flow. For example, ABS at 19 under 10 kg and 220 C does not flow worse than GPPS at 8.0 under 5 kg and 200 C. The numbers sit on different rulers.
How do temperature and load affect MFR?
Higher temperature makes the melt less viscous and easier to flow. Heavier load pushes the material through the die harder. Together they determine the result, so changing either one changes the MFR number.
What does MFR tell me about molecular weight?
High MFR means short molecular chains, low molecular weight, and fewer entanglements. The chains slide past each other easily, like short noodles. Low MFR means long chains that tangle and resist flow, which builds toughness and impact strength.
What is the trade-off of high MFR grades?
High MFR grades fill molds easily and use less energy, but they sacrifice impact strength, elongation at break, melt strength, and resistance to environmental stress cracking. Within one material family, the highest MFR and highest impact grades are almost never the same grade.
How should I read MFR on a data sheet?
Always read MFR together with its temperature and load condition. A sheet showing only “MFR 20” is incomplete. If the sheet cites only a standard such as ASTM D1238 without conditions, treat the number as comparable only within the same grade and batch.
What are common MFR test conditions by material?
High-melting viscous resins such as PC, PA, and PBT use high temperature with light load. PP and PE commonly use 230 C x 2.16 kg or similar light-load tiers. ABS often uses high temperature with heavy load. These tiers follow industry convention.
When should I request same-condition MFR data?
When changing material grades or suppliers. If the conditions do not match, ask for data measured under the same conditions, or run a trial yourself. Do not base a whole batch’s processability on numbers measured differently.