PEEK Properties: 12 Families and 4 Ways They Collapse

Polyether ether ketone (PEEK) properties are set by one molecular decision: three rigid benzene rings, two flexible ether links and one polar ketone in every repeat unit. That arrangement produces a glass transition at 143 degrees Celsius, a melting point at 343 degrees Celsius and roughly 100 MPa tensile strength. It also caps stiffness, notch impact and ultraviolet life. Fillers move part of that envelope and leave the rest untouched.

Why the data sheet stops where the design problem starts

A single tensile number measured at 23 degrees Celsius answers a question that few real parts ask. Parts fail by creep at 150 degrees Celsius, by fatigue after ten million cycles, by a notch that was added for a retaining ring, or by sunlight through a window. None of those appear in the headline row of a table of PEEK material properties.

So the workable way to read PEEK properties is to split them in two. One group belongs to the molecule and cannot be bought back with a filler: glass transition, melting point, dielectric loss, chemical inertness, ultraviolet sensitivity. The other group belongs to the compound and the mold: stiffness retention above the glass transition, wear rate, conductivity, crystallinity. Most specification errors start by mixing the two groups inside one comparison.

The twelve property families in PEEK properties

Twelve families cover every number that follows. Each one answers a different question, and each comes out of a different test.

FamilyQuestion it answersTypical reference method
ThermalHow much temperature before the part loses shape or stiffness?ISO 75 heat deflection at 1.8 MPa; DSC for Tg and Tm
Tensile and flexuralHow much load before yield or fracture at room temperature?ISO 527, ISO 178, ISO 604
Impact and notchWhat happens when the load arrives fast and a stress raiser is present?ISO 179 unnotched and notched Charpy
Creep and fatigueWhat survives 10,000 hours under load, or ten million cycles?ISO 899 constant load; load controlled fatigue
Specific strength and stiffnessIs the part weight limited or deflection limited?Strength or modulus divided by density
Wear and frictionHow fast does material leave the sliding surface?Pin on disc, block on ring, thrust washer (ASTM D3702)
Chemical resistanceWhich media attack it, at what temperature and under what stress?Immersion plus residual strength
Environmental resistanceWhat do sunlight, water, radiation and repeated sterilization do?UV exposure; accumulated gamma dose
ElectricalIs it an insulator, a static dissipator or a conductor?IEC 62631 volume resistivity
FlameDoes it sustain combustion, and at what wall thickness?UL 94 vertical burn; limiting oxygen index
BiocompatibilityCan it sit in tissue, and does bone bond to it?ISO 10993 series
ProcessingDoes the molded part actually carry the properties the grade promises?Mold temperature, crystallinity by DSC, shrinkage

Processing and environmental resistance are the two families most often missing from a specification, and both fail silently in short term testing, which is why they cost the most when they go wrong.

Molecular structure: three rings, two ether links, one ketone

PEEK is a semi-crystalline thermoplastic, and its repeat unit has the empirical formula (C19H12O3)n. That unit contains three para-phenylene rings, two ether links and one ketone group, a ratio of 3 to 2 to 1. Read that ratio as three separate jobs and most of the numbers below explain themselves.

UnitCountWhat it contributesWhat it costs
Para-phenylene ring3Locks chain rotation, lifts Tg and Tm, allows dense packingNothing rotates, so melt viscosity stays high
Ether link2Buys the processing window by holding Tm below the decomposition rangeSoftens the chain relative to a pure ketone backbone
Ketone group1Dipole interaction between chains, so chains enter the lattice on coolingThe carbonyl is also the ultraviolet chromophore

All the rigidity comes from the rings. A benzene ring cannot rotate internally, so segment motion stays frozen until the glass transition unlocks it. The rings also carry no side groups, which is where PEEK differs from a sulfide linked polymer or from the multi-ketone members of the same family. No side groups means tight packing, which is why crystallinity reaches 30 to 40 percent and water uptake stays at 0.1 to 0.5 percent. It also means there is no exposed chemical site for a reagent to attack, and both the solvent resistance and the hydrolysis resistance follow from that.

The two ether links are the ransom paid for processability. A backbone made only of ketone links holds heat better, but its melting point climbs close to the decomposition temperature and the material can no longer be injection molded. A backbone made only of ether links is too soft. PEEK holds the ether to ketone ratio at 2 to 1, which keeps Tm at 343 degrees Celsius, more than 150 degrees below the decomposition range. That gap is the entire injection molding window. The pattern repeats across the whole polyaryl ether ketone family: more ketone means more heat resistance and less processability.

The single ketone group supplies the dipole that makes the chains willing to crystallize. Remove it and the polymer becomes amorphous, in the way that a polyether sulfone is amorphous. Strength would survive, but chemical resistance and fatigue life would drop a full grade.

Two consequences follow the structure everywhere else. The aromatic backbone delivers heat resistance, rigidity, chemical resistance, flame retardancy, low water uptake and no hydrolysis. The semi-crystalline morphology adds fatigue resistance, wear resistance, creep resistance and solvent resistance. The same backbone also imposes three fixed weaknesses: ultraviolet sensitivity, because the rings absorb light and the ketone acts as a photosensitizer; high melt viscosity of 350 to 675 pascal seconds, an order of magnitude above ordinary engineering plastics; and notch sensitivity, because a semi-crystalline polymer has no craze mechanism to spend energy ahead of a crack.

PEEK thermal properties: Tg and Tm belong to the chain, stiffness retention belongs to the filler

The PEEK glass transition temperature and melting point are properties of the molecule, and no filler moves them. What a filler changes is how much stiffness remains once the matrix has softened, and that distinction is the whole story of the thermal table.

PropertyUnfilled30% glass filled30% carbon filled
Glass transition (Tg), degrees Celsius143143143
Melting point (Tm), degrees Celsius343343343
Heat deflection at 1.8 MPa, degrees Celsius152328336
Relative thermal index, electrical, degrees Celsius260240240
Relative thermal index, mechanical with impact, degrees Celsius180not publishednot published
Coefficient of linear expansion45 ppm/Knot published6 ppm/K along flow; up to 100 ppm/K across flow
Thermal conductivity0.29 W/m Knot published0.95 to 2.0 W/m K

The PEEK heat deflection temperature moves from 152 to 336 degrees Celsius, a jump of 184 degrees, and almost nobody reads it correctly. The test asks how hot a specimen gets while still carrying 1.8 MPa of bending stress without deflecting a fixed amount. The unfilled resin loses two to three orders of magnitude of modulus as it crosses Tg, so the bar bends immediately and the reported number is essentially the glass transition. Glass and carbon fibers lock the matrix into a skeletal network, so the composite keeps carrying the bending load after the matrix has softened, and the number climbs into the fiber’s territory.

That is stiffness retention, not a higher service temperature. Filler shares the load; it does not stop chain motion. Above 143 degrees Celsius the unfilled matrix still collapses, and the fiber simply carries a larger and larger fraction of the stress. The long term measure that means something is the PEEK relative thermal index: 260 degrees Celsius for electrical use and 180 degrees Celsius where mechanical impact applies, and that is the published long term commitment. HDT is not.

One counterintuitive consequence of the same table: reinforced grades carry a lower electrical relative thermal index, 240 degrees Celsius, than the unfilled resin at 260. The filler interface becomes the weak point under sustained heat. If the application is long term electrical insulation above 250 degrees Celsius, the unfilled grade is the more conservative choice, not the reinforced one.

Reinforcement brings three side effects. Thermal expansion becomes strongly anisotropic: 6 ppm/K along the flow direction is below a quarter of aluminum at 23 ppm/K, while the transverse direction can reach 100 ppm/K, so a long part grows almost nothing in one direction and grows fast in the other, and warps. Thermal conductivity spans an order of magnitude, from 0.29 W/m K, effectively an insulator, to between 0.95 and 2.0 W/m K in a carbon grade. That is helpful in a bearing where friction heat must escape and harmful in a thermal break.

PEEK mechanical properties: yield is not fracture and flexure is not tension

The sentence “PEEK has 100 MPa tensile strength” hides two different measurements. In the unfilled grade, 100 MPa is the yield strength; fracture occurs near 110 MPa. Reinforced grades barely yield at all, so only a fracture value is quoted. Comparing a yield number from one grade against a fracture number from another produces nonsense, and it shows up in a surprising number of supplier charts.

PropertyUnfilled PEEK
Tensile strength at yield100 MPa
Tensile strength at break110 MPa
Flexural strength165 MPa
Compressive strength125 MPa
Tensile modulus3.7 GPa (above 12 GPa with carbon fiber)
Flexural modulus3.8 GPa
Elongation at break40 to 45 percent

Flexural strength sits 65 percent above tensile strength. The mechanism is mechanical, not chemical: in bending, one face is in compression and the other in tension while material near the neutral axis never reaches its limit, and compressive strength at 125 MPa is already higher than tensile. The design implication is blunt. A load carried in bending, through a cantilever, a simply supported beam or a snap fit, has more margin than the same load carried in tension. Failure analyses of PEEK parts regularly find that the designer sized a bending member against tensile data and left 60 percent of the margin unused. The reverse mistake is more dangerous: sizing a tension member from flexural data.

Test system matters as much as test geometry when PEEK properties are compared across suppliers. ASTM and ISO values for the same grade differ by a few percent and do not always move in the same direction. One unfilled grade reads 97 MPa in tension under ASTM and 170 MPa in flexure, against 100 and 165 under ISO. Mixing the two systems inside one comparison table is a common and quiet error.

Temperature is where the real cliff sits.

TemperatureFlexural strength, unfilledFlexural strength, 30% carbon
Room temperature165 MPanot stated
125 degrees Celsius85 MPa160 MPa
175 degrees Celsius19 MPa85 MPa
Above 175 degrees Celsius12.5 MPanot stated

From 125 to 175 degrees Celsius the unfilled grade loses 78 percent of its flexural strength. That is the glass transition at work, and it behaves like a step rather than a slope. The carbon grade loses 47 percent over the same interval, because the fiber already carries most of the load. The unfilled series is the clearest argument in the whole property set for treating 143 degrees Celsius as a hard design line rather than a soft one.

PEEK notched impact strength: the test that flatters the material

PEEK impact data come as a combination that misleads almost everyone who reads only the first row.

SpecimenResult
Unnotched CharpyNo break; the specimen survives to the end of the pendulum travel
Notched, unfilled7 kJ/m2
Notched, 30% glass filled10 to 11 kJ/m2
Notched, 30% carbon filled7.0 kJ/m2

“Unnotched: no break” reads like an exceptionally tough material. The same batch, with one standard notch cut into it, drops to 7 kJ/m2, which is below several general purpose engineering plastics. Both readings are correct. Without a stress concentration, PEEK absorbs energy through large scale yielding across a 40 to 45 percent elongation at break. With a notch, stress concentrates at a single point and a semi-crystalline polymer has no craze mechanism to spread the damage, so it fractures in a brittle mode.

Carbon fiber does not fix this, and the reason is worth remembering. The fiber to matrix bond in a carbon composite is strong, so a crack that starts at a notch runs straight through the fiber instead of pulling it out. Carbon itself is brittle and breaks with a flat face, so no energy is spent on debonding or pull out. Glass has a weaker interface, which allows debonding and fiber pull out to absorb energy, and that is why the glass grade reaches 10 to 11 kJ/m2 while the carbon grade returns to 7.0.

The selection rule is counterintuitive, and it gets ignored constantly. If a part has to survive impact, do not default to the carbon grade. Carbon buys modulus, strength, wear resistance and electrical conductivity. It does not buy toughness, and it leaves notch sensitivity exactly where it was.

Low temperature is the one place where PEEK behaves better than intuition suggests. At minus 40 degrees Celsius, and even in liquid nitrogen at minus 196, it does not embrittle the way polycarbonate or acrylic does. Below the glass transition there is little segment motion left to freeze, and the crystalline regions keep supporting the structure. Cryogenic sealing and cold structure applications are therefore reasonable. Notch sensitivity, however, does not improve with cold, so low temperature operation should not be read as extra toughness.

PEEK creep resistance and fatigue: the strength that survives ten thousand hours

A short term tensile test reports the load needed to break a specimen. Real parts are rarely broken. They deform slowly under a steady load, or crack slowly under a repeating one. Those two behaviors set the real service limit, and they are the part of the PEEK properties set that a supplier is least willing to publish.

ConditionCreep strainReading
200 degrees Celsius at 10 MPaJust over 1 percentLow stress, high temperature: 10 MPa is a tenth of room temperature strength
150 degrees Celsius at 35 MPa2 to 3 percentOutside tolerance for a part held to plus or minus 0.05 mm

The 200 degree row looks reassuring and is close to meaningless for structural work, because 10 MPa is far below any realistic design stress. The 150 degree row is the honest one. Two to three percent strain on a 20 mm dimension is 0.4 to 0.6 mm of movement, an order of magnitude beyond a precision tolerance, and no amount of grade selection removes it. Geometry, wall thickness and fiber loading are the only levers.

Stress relaxation is the same phenomenon seen from the other side, and bolted joint design routinely forgets it. A PEEK bolted joint at elevated temperature loses 15 to 25 percent of its preload over the first 1,000 hours, after which the curve flattens. The workable rule is to reserve that loss up front and design the joint against the plateau rather than the initial torque. A metal bolt in the same joint loses under 5 percent, which is why the metal design habit does not transfer.

Fatigue numbers for PEEK circulate in three different ranges, and the conflict is usually a reporting error rather than a data error.

LoadingMean stressFatigue limit at 10 million cycles
Fully reversed flexureR = -141 to 48 MPa
Tension to tensionR above 050 to 60 MPa
Gear tooth contactComponent level, triaxial compressionHigher; not comparable to coupon data

The PEEK fatigue limit depends strongly on mean stress. Fully reversed loading is the most severe case and gives the lowest limit. Tension to tension loading keeps a mean tensile stress but a smaller amplitude, so the limit rises. Gear data sit higher again because a gear tooth is a component tested under three dimensional compression at the contact, which is not the same stress state as a uniaxial coupon test.

So match the PEEK properties to the load history. Rotating shafts and reciprocating rods see symmetric alternating stress, so design to 41 to 48 MPa at ten million cycles and then apply a safety factor. Pressure cycling and on off actuation are pulsating, so 50 to 60 MPa is available. Gear tooth data should never be used to size a coupon level part.

PEEK outperforms most polymers in fatigue for a structural reason: a fatigue crack has to cross the crystalline lamellae, and each lamella acts as a barrier in front of the crack tip. That is why its fatigue limit reaches 40 to 50 percent of static strength, while polystyrene and acrylic typically manage 20 to 30 percent. The trade is that once a crack does start, from a notch or a machining mark, it propagates faster than expected. Fatigue design for PEEK therefore concentrates on preventing initiation rather than resisting growth, which puts surface finish, fillet radius and residual stress ahead of material selection.

Specific strength and specific stiffness: the comparison with aluminum that keeps being misused

“PEEK has eight times the specific strength of aluminum” is one of the most repeated claims about PEEK properties, and one of the most widely misapplied. Two separate ratios are involved, and they point in opposite directions.

MaterialSpecific strengthSpecific stiffness
Unfilled PEEK773.1
30% carbon filled PEEK16520
Aluminum alloy11025.6
304 stainless steel70not published

On specific strength, unfilled PEEK at 77 already beats 304 stainless at 70, and the carbon grade at 165 beats aluminum at 110. The claim survives, but it is clearest for the carbon grade; unfilled resin is roughly level with aluminum rather than far ahead.

On specific stiffness the result reverses. Unfilled PEEK at 3.1 against aluminum at 25.6 is a factor of eight behind, and even the carbon grade at 20 stays below aluminum. A like for like section swap from aluminum therefore keeps the strength and loses the stiffness. Deflection rises by five to eight times, which shows up as fit clearance change, seal failure, amplified vibration and lost positioning accuracy, not as a broken part.

The fix is an equal stiffness design rather than an equal section design. Increase the second moment of area with ribs, thicker walls, or an I or box section, or move to the carbon grade. After that change, weight still falls by 40 to 60 percent, but the reduction comes from the geometry, not from the material swap alone.

There is a second layer. Specific strength is calculated from fracture, while most engineering parts are governed by deflection. For a deflection controlled part, specific stiffness is the real metric, and the PEEK advantage shrinks sharply. Specific strength only becomes the deciding number where weight reduction is mandatory and larger deflection is acceptable: airborne brackets, robot joints, handheld device housings.

PEEK wear resistance and friction: the base resin is a starting point

“PEEK is wear resistant” needs a long qualification, longer than any other branch of PEEK properties. Under dry sliding against steel, unfilled PEEK is a mid range material with a friction coefficient of 0.32 to 0.36, worse than several filled engineering plastics. Its real value in tribology is as a matrix that can carry a wear package at 250 degrees Celsius, which no commodity polymer can do.

Three fillers do three different jobs, and a package needs all of them.

FillerTypical loadingJobBoundary
Carbon fiber10 to 30 percentCarries contact stress; fiber ends meet the counterface first and shield the softer matrix from plowingBecomes abrasive at high loading and scratches soft counterfaces
PTFE10 to 20 percentBuilds a transfer film during run in, turning PEEK on steel into PTFE on PTFECosts strength and creep resistance, so only a minority addition works
GraphiteModerateConducts heat and lubricates when dry and hotFails in the presence of water

Limiting PV values for PEEK appear across a range from 0.14 to 31,400 psi ft per minute, which looks like fabricated data and is not. Three mechanisms explain the spread. Unit conversion alone accounts for 28,500 fold, since 1 MPa m/s is about 28,500 psi ft per minute. Failure criteria differ, and wear through, friction coefficient breakaway and interface melting give answers that differ by several times. Test geometry differs, and a thrust washer, a block on ring and a pin on disc have completely different heat removal paths.

PV values can be compared inside one method and one failure criterion, and nowhere else. For a real application, run the target contact condition, or use the supplier’s application window measured in the same geometry.

Three variables get left out of wear specifications. Counterface material decides everything: carbon filled grades perform best against hardened steel above 58 HRC, and act like sandpaper against soft metals such as aluminum. Water changes the ranking: a PTFE package loses its transfer film to water and wear rate rises three to four times, while a carbon package rises by about 30 percent, so wet service should default to carbon, not PTFE. Annealing is the third. An unannealed carbon and PTFE grade wears at about 0.85 in the test’s own units, and after a full anneal at 160 to 180 degrees Celsius that raises crystallinity to 33 percent, the rate falls to about 0.45 and limiting PV improves by roughly 20 percent. For a wear part, annealing is not an optional finishing step. It is part of the specification.

PEEK chemical resistance: broad coverage with three hard edges

PEEK resists chemicals because it offers no point of attack, which makes chemical resistance the one PEEK properties claim that rests on the backbone rather than on the compound. The backbone is fully aromatic, with no ester, amide or hydroxyl group and no side chains, so hydrolysis, oxidation, acid attack and base attack all lack an entry point. Broad coverage is not universal coverage, and the exceptions cluster in strongly oxidizing and strongly protonating media.

Concentrated sulfuric acid is the standard test case, and the literature appears to contradict itself. Most resistance tables list it as unsuitable, yet measured data exist showing 98 percent acid at 25 degrees Celsius for 30 days producing less than 0.5 percent weight gain and no strength loss. Both statements hold, because degradation is slow at ambient temperature and accelerates with heat. At room temperature a short exposure sulfonates the surface only, and the bulk is untouched. Above roughly 50 degrees Celsius, or over a long enough time, the sulfonated layer moves inward and the part eventually embrittles.

So the engineering statement needs its conditions attached: acceptable at ambient temperature, short term and unstressed; not acceptable hot, long term and under stress. Any claim that PEEK completely resists or completely fails in concentrated sulfuric acid has dropped the conditions.

Standard chemical resistance testing immerses an unstressed specimen, then weighs it and measures residual strength. Real parts sit in the medium while carrying load, which is environmental stress cracking. PEEK sits in the good tier for stress cracking resistance among engineering plastics, but concentrated sulfuric acid or a strong polar solvent combined with high residual stress at a gate or a thread root can still produce cracks. Annealing at 190 to 200 degrees Celsius to relieve molded in stress, plus avoiding sharp corners and abrupt section changes, removes most of that risk.

Environmental resistance: hydrolysis and radiation hold up, ultraviolet does not

Describing PEEK as having excellent weathering resistance is the most common error in the PEEK properties literature, and the careful sources are more cautious than the marketing. PEEK is not especially ultraviolet tolerant, and long outdoor exposure needs a UV stabilizer, a carbon black filled grade or a protective coating.

The reason sits in the structure rather than in the processing. The backbone is a conjugated phenyl ether phenyl ketone system, and the rings absorb strongly between 300 and 350 nm, which is exactly the UV-B to UV-A band of the solar spectrum. After absorbing a photon the ketone acts as a photosensitizer and undergoes Norrish type photolysis, generating radicals that attack the ether links. Chain scission, crosslinking and surface oxidation follow. The visible sequence runs from color shift and darkening of the beige surface, to chalking, to loss of surface mechanical properties, then inward.

Carbon filled grades look more weather resistant, but that is the carbon black and the fiber absorbing and shielding the light, not an improvement in the matrix. A black carbon loaded grade does outlast a natural grade outdoors for the same reason.

Three environmental boundaries are easy to miss. Strong oxidizing cleaners used in food and semiconductor plants, including peracetic acid, ozonated water and piranha solution, attack the surface and leave it oxidized and rough. Oxygen at 250 degrees Celsius over long periods raises melt index and drops mechanical properties by 30 to 50 percent, while inert atmosphere or a sealed oxygen free enclosure extends life considerably. Repeated sterilization accumulates: a single gamma dose is harmless, but more than 50 cycles may approach the material’s tolerance, so the assessment should use total dose rather than dose per cycle.

PEEK electrical resistivity: eleven orders of magnitude inside one family

Electrical behavior is where a good matrix gets ruined, or repurposed, by a filler, more clearly than anywhere else in the PEEK properties set. Unfilled PEEK is close to an ideal insulator. Add carbon fiber and it becomes a conductor. That is not a defect; it is a different product category.

GradeVolume resistivityTypical use
Unfilled10^16 ohm cmHigh voltage insulation, semiconductor test sockets, connector bodies
Antistatic and wear grades10^10 ohm cmTrays and fixtures that drain static without conducting
Carbon filled10^5 ohm cm; surface resistance as low as 10^3 ohmEMI shielding housings, conductive parts in explosive atmospheres

Eleven orders of magnitude separate those rows, which is enough for one material family to serve applications that share nothing. The unfilled figure also moves with temperature: 10^16 ohm cm at room temperature, 10^15 at 125 degrees Celsius and 10^9 at 275 degrees Celsius. Seven orders of insulation are lost between ambient and the top of the range, and any high voltage hot application has to calculate with the hot value.

Dielectric constant follows the same mechanism. It reads 3.0 at 23 degrees Celsius and 4.5 at 200 degrees Celsius, a 50 percent rise, because segmental motion above the glass transition increases polarizability. For high frequency circuits, radomes and antenna substrates, that drift changes resonant frequency and impedance matching directly. Dissipation factor stays low at around 4 x 10^-3 even at temperature, which is the property that makes PEEK usable as a high frequency substrate at all.

Flame retardancy: V-0 without a single additive

PEEK reaches UL 94 V-0 with no flame retardant package, and that is why it holds a distinct position in aviation, rail and semiconductor equipment. The rating comes from the structure, not the formulation.

Three mechanisms stack, and all three come out of the same backbone, which is why the rating needs no formulation work at all. The high aromatic content drives char formation on burning, and the char layer insulates the underlying material from heat and oxygen. The high melting point and high melt viscosity prevent dripping, and dripping is what spreads fire in most plastics. The limiting oxygen index of 35 percent means combustion needs 35 percent oxygen to sustain itself, against 21 percent in air, so the material self extinguishes.

Reinforcement improves the rating further, because glass or carbon fiber forms a skeleton that suppresses melt drip. A reinforced grade reaches V-0 at 0.5 mm wall, while the unfilled resin needs 1.5 mm. Thin wall flame retardant parts should therefore start from a reinforced grade.

Biocompatibility: inert in both directions

PEEK is one of the most successful polymers in implantable devices, and roughly half the global interbody fusion cage market uses it, which makes biocompatibility the most commercially proven branch of PEEK properties. It works by a different mechanism from titanium’s. Tissue does not recognize PEEK; tissue accepts titanium. That difference generates both the clinical advantages and the technical problems.

Four advantages follow from the structure. Flexural modulus is 3.8 GPa against 10 to 20 GPa for cortical bone and about 110 GPa for titanium alloy, so PEEK is nearly 30 times less stiff than titanium and is the closest commercial implant material to bone. Stress shielding falls accordingly, and reported subsidence for PEEK cages is below 10 percent against 20 percent or more for titanium. The material is radiolucent under X-ray, CT and MRI, so bone fusion around the implant is visible without metal artifact, and barium sulfate can be added when visibility is needed without significant mechanical cost. It is chemically inert and does not degrade, releasing no monomer and no acidic by product, with more than 20 years of clinical follow up behind it. It also survives repeated gamma, electron beam, ethylene oxide and steam sterilization.

The cost of that inertness is that PEEK neither rejects nor integrates. The surface is hydrophobic with low surface energy, so protein adsorption and cell adhesion are both poor. Bone forms a fibrous tissue layer against the implant instead of bonding to it, which appears on CT as a halo around the device. Fusion is slower than with titanium. Four routes address it: hydroxyapatite coating, plasma or acid etching to raise surface energy, blasting or porosifying the surface, and carbon fiber reinforced PEEK; a titanium coating on a PEEK substrate is a newer hybrid that trades some radiolucency for osseointegration.

Wear debris deserves a separate question for load bearing implants. Unfilled PEEK is a mid range wear material, so articulating surfaces usually move to carbon fiber reinforced PEEK, and the regulatory question is whether carbon wear particles provoke inflammation. The accepted control is particle size: keep fiber length and distribution so that debris lands at or above 10 micrometers, a size macrophages can clear without chronic inflammation. A buyer should ask for the particle size distribution and the full ISO 10993 data set, distinguish medical grade from industrial grade of identical chemistry, require a batch certificate of analysis with DSC curve, ash content and molecular weight distribution, and confirm sterilization method and cycle count.

Processing: mold temperature decides more than the grade does

PEEK is not difficult because the temperatures are high. It is difficult because four separate temperature windows have to be right at once: drying, melt, mold and anneal. Get any one wrong and the part looks acceptable and performs as a different material.

Mold temperature sits between 170 and 205 degrees Celsius, and that single number controls about 40 percent of the delivered properties, because crystallinity is set by cooling rate. Below the glass transition the melt freezes as it enters the cavity, the chains never reach the lattice, and the result is an amorphous or low crystallinity part. It looks normal and measures to dimension, but strength is only 60 percent, stiffness 50 percent and chemical resistance 20 percent of the specified values.

Conventional inspection cannot see that failure. Appearance, dimensions and even short term tensile tests can pass, and only long term chemical, fatigue and wear testing exposes it. The practical consequence is equipment: PEEK molding needs oil temperature controllers running at 180 to 220 degrees Celsius and hot work tool steel, which ordinary water cooled tooling cannot deliver. The investment threshold for a PEEK line is a different order from a line running ABS.

Shrinkage adds a second trap. A carbon filled grade shows roughly 5 to 1 anisotropy, shrinking near zero in one direction and about 0.5 percent in the other, so a long part warps rather than shrinking uniformly. Mold design needs flow simulation, or machining allowance on critical dimensions followed by a finishing cut.

Machined parts have their own rule. Extruded rod and plate carry orientation stress from the extrusion, and milling releases it, so the part moves after the cut and tolerance is lost. The standard practice is to anneal at 190 to 200 degrees Celsius for 2 to 4 hours before machining, and to run a second stress relief after machining where tolerance is tight.

Crystallinity is a design variable rather than a fixed property. Slow cooling in a hot mold or a thick wall gives 35 to 40 percent crystallinity, which improves wear resistance, chemical resistance and creep resistance at the cost of ductility. Fast cooling in a cold mold or a thin wall gives lower crystallinity, better toughness, weaker chemical and wear performance. One grade can therefore be tuned to different property sets by process alone, which means a drawing that says only “material: PEEK” has not specified the part. Wear and chemical applications should carry an explicit crystallinity and annealing requirement.

Selection: matching the grade to the failure mode

Failure mode or requirementStarting pointReason
Long term electrical insulation above 250 degrees CelsiusUnfilledHighest electrical relative thermal index at 260 degrees Celsius
Thin wall flame retardanceGlass or carbon filledV-0 at 0.5 mm instead of 1.5 mm
Wear in water or wet lubricantCarbon filled, no PTFEPTFE transfer film is washed away and wear rises three to four times
Dry wear against hardened steelCarbon plus PTFEContact stress support plus low friction
EMI shielding or static dissipationCarbon filled10^5 ohm cm, surface resistance to 10^3 ohm
Impact loaded partUnfilled or glass filledCarbon leaves notched impact unchanged at 7 kJ/m2
ImplantMedical grade unfilled, or CFR-PEEK after particle reviewPurity, traceability, ISO 10993 data
Precision part with tight toleranceHigh mold temperature plus annealCrystallinity and stress relief control the final dimension
Weight critical with deflection allowedCarbon filled with equal stiffness geometrySpecific strength 165 against 110 for aluminum

The counterintuitive part: four places where PEEK properties disappear

Four conclusions run against the sales pitch, and all four fall out of the same tables.

The heat deflection jump is stiffness retention, not a higher ceiling. A part rated 336 degrees Celsius on HDT still loses 78 percent of its flexural strength between 125 and 175, because the matrix is a matrix at every temperature.

Carbon fiber buys modulus, not toughness. Notched impact stays at 7.0 kJ/m2, the same as unfilled resin, and the part becomes electrically conductive at 10^5 ohm cm and starts scratching aluminum counterfaces. Three regressions accompany one improvement.

A cold mold halves the material without leaving evidence. Sixty percent strength, fifty percent stiffness and twenty percent chemical resistance, with dimensions and short term tests passing, is the most expensive defect in the family because nothing catches it at goods inwards.

An equal section swap from metal makes the part softer. Specific stiffness at 3.1 against 25.6 for aluminum is a factor of eight, and the resulting deflection of five to eight times shows up as a functional failure rather than a structural one.

Limitations

Everything here is a typical value at grade level, not a qualification for any specific part. ISO and ASTM systems differ by a few percent and not always in the same direction, so a comparison should stay inside one system. Creep and fatigue data scatter with mean stress, surface condition, frequency and specimen geometry, and the fatigue range from 41 to 48 MPa assumes a polished coupon. Wear and PV data are only comparable within one method and one failure criterion, and the wear figures quoted here come from dry sliding against hardened steel at ambient temperature. Chemical resistance depends on temperature, exposure time and applied stress, and the sulfuric acid behavior changes qualitatively above about 50 degrees Celsius. The flexural series for the unfilled grade is reported as four readings without a label on the last point, and the reinforced series is shorter than the unfilled one, so the high temperature comparison is indicative rather than complete. None of this replaces a coupon test in the actual medium at the actual stress.

Bottom line

PEEK properties are a set of trades rather than a set of strengths. Fiber buys stiffness and gives up toughness. Lubricant buys wear resistance and gives up strength. Higher crystallinity buys chemical resistance and gives up ductility. A cold mold buys appearance and gives up almost everything else.

So the method is not to hunt for the strongest grade. It is to name what the part fears most, which might be creep at 150 degrees Celsius, a notch, ultraviolet light, a wet counterface or a 0.05 mm tolerance, and then deliberately give up the properties that do not matter. Almost every expensive PEEK failure can be traced to a specification that tried to keep all of them.

FAQ

What is PEEK made of?

PEEK is a linear aromatic thermoplastic whose repeat unit holds three para-phenylene rings, two ether links and one ketone group, giving the empirical formula (C19H12O3)n. The rings supply rigidity and heat resistance while the ether links keep the melting point low enough for injection molding. With no side groups, chains pack tightly and water uptake stays between 0.1 and 0.5 percent.

Why does heat deflection rise from 152 to 336 degrees Celsius with fiber?

Heat deflection is the most misread number in the PEEK properties set: it measures how hot a specimen gets while carrying 1.8 MPa of bending load. Unfilled resin softens at its glass transition and deflects at 152 degrees Celsius, while fiber holds the matrix in a skeleton and keeps the composite stiff to 336. That is retained stiffness, not a higher service temperature: the matrix still softens at 143.

Is PEEK stronger in bending than in tension?

Yes, by about 65 percent. Unfilled PEEK reaches 165 MPa in flexure against 100 MPa at tensile yield, because bending loads part of the section in compression and leaves material near the neutral axis below its limit. That margin rewards cantilever and snap fit designs, but sizing a tension member from flexural data is unsafe.

Does carbon fiber improve notched impact strength in PEEK?

No. A 30 percent carbon filled grade measures 7.0 kJ/m2 notched in a standard Charpy test, the same as unfilled resin, while a glass filled grade reaches 10 to 11. Carbon bonds strongly to the matrix, so a crack crosses the fiber instead of pulling it out, and carbon itself is brittle, while glass debonds and dissipates energy.

How much does PEEK creep at 150 degrees Celsius?

At 150 degrees Celsius and 35 MPa, unfilled PEEK accumulates 2 to 3 percent creep strain over the test period. On a 20 mm dimension that is 0.4 to 0.6 mm of movement, far outside a tolerance of plus or minus 0.05 mm. A 200 degree reading of just over 1 percent looks better only because 10 MPa is a tenth of room temperature strength.

What is the fatigue limit of PEEK at ten million cycles?

Fully reversed loading gives 41 to 48 MPa at ten million cycles, the conservative figure for rotating shafts and reciprocating rods. Tension to tension loading raises the limit to 50 to 60 MPa because the stress amplitude is smaller. Gear tooth data run higher still but come from component tests under triaxial compression, so they cannot size a coupon level part.

Is PEEK stiffer than aluminum?

No, and the gap is wide. Specific stiffness for unfilled PEEK is 3.1 against 25.6 for aluminum, a factor of eight, and even a 30 percent carbon grade at 20 stays below aluminum. Strength per unit weight does exceed aluminum in the carbon grade, but an equal section swap still makes a part deflect five to eight times more under the same load.

Is unfilled PEEK a good wear material?

Only in a narrow sense, because wear is the one branch of PEEK properties decided by the compound rather than the resin. Dry against hardened steel, unfilled PEEK shows a friction coefficient of 0.32 to 0.36 and wears faster than several filled engineering plastics. Its real value is as a matrix that can carry carbon fiber, PTFE and graphite at 250 degrees Celsius.

Can PEEK handle concentrated sulfuric acid?

At 25 degrees Celsius for 30 days, 98 percent sulfuric acid produces less than 0.5 percent weight gain and no strength loss in unstressed coupons. Above about 50 degrees Celsius the sulfonated layer moves inward and the part embrittles. The defensible rule is ambient, short term and unstressed, and never hot, long term or under load.

Is PEEK resistant to ultraviolet light?

No. Ultraviolet is the weakest branch of PEEK properties, and the mechanism is structural rather than incidental. Aromatic rings absorb strongly between 300 and 350 nm, the ketone acts as a photosensitizer, and radicals attack the ether links, so surfaces darken, chalk and lose mechanical properties from the outside in. Outdoor parts need carbon black, a UV stabilizer or a coating.

Is PEEK biocompatible?

PEEK passes ISO 10993 and holds more than 20 years of clinical use, plus roughly half the global interbody fusion cage market. Its 3.8 GPa flexural modulus is close to cortical bone and nearly 30 times below titanium alloy, which limits stress shielding and holds subsidence below 10 percent. The same inertness stops bone bonding directly, so fusion depends on hydroxyapatite coating or surface roughening.

Why does mold temperature matter so much for PEEK?

Crystallinity is set by cooling rate, so mold temperature between 170 and 205 degrees Celsius decides how much of the promised PEEK properties arrive in the part. Below the 143 degree glass transition the melt freezes amorphous and delivers 60 percent strength, 50 percent stiffness and 20 percent chemical resistance. Dimensions and short term tensile tests pass, so only long term testing exposes it.