Plastic identification methods work by elimination rather than by a single test. You narrow the candidate list with a density reading, a solubility check and a heating observation, screen for heteroatoms, then confirm the polymer with FTIR, adding DSC or TGA when thermal behavior carries the argument. No single test establishes identity on its own, and knowing the polymer class is not the same as knowing the grade.
What plastic identification methods actually have to answer
“Which plastic is this?” contains three separate questions, and they need very different amounts of work.
Table 1. The three questions that plastic identification methods are asked to answer.
| Level | Question | What answers it | What it still leaves open |
| 1. Polymer class | Is this PE, PP, ABS, PC, PA, POM, or a fluoropolymer such as PTFE, FEP, PFA or PVDF? | Density, heating behavior, FTIR | Additives, fillers, grade |
| 2. Composition | What else is in the part, such as pigment, filler, flame retardant, impact modifier or stabilizer? | Ash content, TGA, SEM-EDS, XRF | The molecular structure of each additive |
| 3. Grade or specification | Does the material meet a named grade or a customer specification? | Melt flow rate, molecular weight distribution, mechanical testing, full formulation data | Nothing, provided the test plan is complete |
A glass fiber reinforced PA and an unfilled PA belong to the same polymer class, yet they differ in density, mechanical performance, processing behavior and ash residue. Black plastic containing carbon black can share its base resin with an uncolored sample and still differ in color, conductivity and thermal response. Two samples confirmed as PP are not automatically the same grade, because melt flow rate, molecular weight distribution, additive package, crystallization behavior and mechanical properties can all diverge.
So the rule is straightforward. Identifying the polymer class does not determine the full formulation, and determining the polymer family does not confirm a commercial grade. If the only question is roughly which family an unlabeled pellet belongs to, a screening pass may be sufficient. If purchasing, a quality dispute or a field failure is involved, the analysis has to be more complete.
The method families in plastic identification
Every family below observes one property. Put them side by side and you can see why plastic identification methods get combined rather than chosen, and where each one stops being useful.
Table 2. Method families, the question each one answers and its main limitation.
| Method family | Question it answers | Typical output | Main limitation |
| Visual and physical inspection | Is the part thermoplastic or thermoset, filled or unfilled, foamed or solid? | Descriptive record | Strongly operator dependent |
| Solubility and swelling | Does the polymer dissolve, swell or stay inert in a given solvent? | Solvent response class | Crosslinked and semi-crystalline grades behave unpredictably |
| Density | Which density band does the material fall into? | g/mL value or sink and float result | Overlapping ranges and fillers blur the answer |
| Heating behavior | How does the sample respond to pyrolysis, burning and melting? | Flame, drip, odor and residue notes | Additives dominate what you observe |
| Heteroatom tests | Are nitrogen, chlorine, sulfur or fluorine present? | Elemental presence or absence | Element presence is not a chemical identity |
| Classification analysis | Which candidate family should be tested next? | Reduced candidate list | A framework, not a measurement |
| Specific identification reactions | Does a characteristic color or reaction product appear? | Supporting evidence only | Poor selectivity and heavy additive interference |
| FTIR | Which functional groups are present? | Absorption spectrum matched to references | Blends, coatings and degradation confuse matching |
| DSC | At what temperature does the material melt, crystallize or soften? | Transition temperatures and enthalpies | Thermal history shifts the curve |
| TGA | How does mass change with temperature in a set atmosphere? | Decomposition steps, volatile content, residue | Residue is not automatically filler content |
| SEM-EDS | What does a particle look like and which elements are in it? | Morphology image plus elemental map | Elements only, no compound identification |
| XRF | Which elements are present in the bulk or on a surface? | Rapid multi-element screen | Says nothing about polymer structure |
Why structure and sample preparation decide the result
Polymers separate in these tests because their molecular structures differ. Polyethylene chains are built mainly from carbon to carbon and carbon to hydrogen bonds. Polyamides carry amide groups, polycarbonates carry carbonate linkages, and polyoxymethylene repeats an oxygen-containing segment. Those structural differences propagate into density, dissolution behavior, thermal transitions, chemical reactivity and infrared spectra.
PE and PP are both polyolefins, so some chemical features sit close together, yet density, melting behavior and infrared features still separate them. PA6 and PA66 share a functional group, but their repeat units and thermal behavior differ. Closely related materials like these need several indicators acting together, which is why one test is never enough on its own.
Sample preparation carries as much weight as the measurement does. Oil, release agents and other surface contamination interfere with surface infrared analysis. Uneven filler distribution means a small local sample may not represent the whole part. Material that has been through long high-temperature processing has a chemical structure and thermal behavior that differ from the virgin resin.
Work out where the sample came from and what state it is in before analysis starts. With pellets, check for mixed resin, moisture and contamination. With pipe, film and molded parts, consider whether skin and core differ. With an exudate that appears during production, separate the abnormal phase from the bulk material and analyze it as its own object.
A white deposit on a pipe cannot be called FEP simply because the pipe is FEP. The deposit may come from the polymer, an additive, an external contaminant or equipment residue, and only analysis of the deposit itself narrows that down. Sample preparation exists to guarantee that the object you test matches the question you are asking.
Solubility testing: dissolution, swelling and surface change are three different outcomes
Solubility has been an observation point in plastics analysis for a long time. Polymers differ in molecular structure, crystallization behavior and intermolecular interaction, so their response to a given solvent differs too. Some dissolve under the right conditions, some swell, and some resist the solvent almost completely.
Those three outcomes must be kept apart.
- Dissolution means the material forms a uniform molecular or polymer solution.
- Swelling means solvent enters the polymer and the volume increases, without the material necessarily dissolving.
- Surface change may be nothing more than softening, cracking or another physicochemical change at the surface, and does not count as dissolution.
Partly crosslinked polymers can swell without ever dissolving the way a linear polymer does. With semi-crystalline plastics, dissolution depends on crystallinity, molecular weight and test conditions as much as on molecular structure. A material that fails to dissolve in one solvent is therefore not assigned to any particular class by that result alone. Solubility testing is best used to exclude candidates or to generate leads for later analysis.
Solvent choice, temperature control and handling all carry chemical risk. Unknown samples should not be exposed to aggressive reagents, toxic solvents or high-temperature chemical treatment on a guess. That work belongs in a laboratory with containment and waste handling in place.
Density testing: the fastest way to cut a candidate list
Density is a basic physical parameter and one of the easiest identification signals to obtain in a plant. PE and PP sit at the low end of the common plastics. PS, ABS, PC, PA and POM are higher. PTFE is among the denser polymers in routine industrial use.
Table 3. Starting density and melting windows for common unfilled thermoplastics. These are typical public material data ranges for laboratory screening, not grade specifications, and not a guarantee for any supplier’s product.
| Polymer | Typical density (g/mL, unfilled) | Typical melting range (degrees Celsius) | Notes |
| PP | 0.89 to 0.91 | 160 to 170 | Floats in water |
| PE, LDPE through HDPE | 0.91 to 0.96 | 105 to 135 | Floats in water |
| PS | 1.04 to 1.06 | Amorphous, no melting point | Glass transition near 100 degrees Celsius |
| ABS | 1.04 to 1.07 | Amorphous | Acrylonitrile, butadiene and styrene terpolymer |
| PA6 | 1.12 to 1.15 | 215 to 225 | Density shifts with crystallinity and moisture pickup |
| PA66 | 1.13 to 1.15 | 255 to 265 | Overlaps PA6 on density |
| PMMA | 1.17 to 1.20 | Amorphous | Glass transition near 105 degrees Celsius |
| PC | 1.19 to 1.22 | Amorphous | Glass transition near 145 to 150 degrees Celsius |
| PET | 1.33 to 1.40 | 250 to 260 | Crystalline and amorphous grades differ |
| Rigid PVC | 1.35 to 1.45 | Amorphous | Plasticized grades sit far lower |
| POM | 1.40 to 1.42 | 165 to 175 | High crystallinity |
| PVDF | 1.76 to 1.79 | 165 to 175 | Fluoropolymer |
| FEP and PFA | 2.12 to 2.17 | 260 to 310 | Fluoropolymers |
| PTFE | 2.14 to 2.20 | 325 to 330 | Does not flow above its melting point |
Water at 1.00 g/mL is the natural first reference. An unknown sample that floats is very likely a polyolefin; one that sinks well below the common polyolefin range widens the candidate list again rather than narrowing it to one answer. Beyond a simple sink and float check, ISO 1183 and ASTM D792 define how the measurement is made, and a density gradient column or pycnometer gives a number instead of a band.
Density still cannot settle identity by itself. The PE and PP ranges can come close, particularly in modified grades. PA6 and PA66 overlap. Glass fiber, calcium carbonate and titanium dioxide fillers shift density substantially, so a filled compound can land nowhere near the range listed for its base resin. Density narrows the field; it does not return one answer.
Heating behavior: pyrolysis, burning and melting are three different tests
How a plastic responds to heat is a substantial part of traditional identification, but pyrolysis, burning and melting behavior are not the same measurement and should not be reported as if they were.
Table 4. Three heating observations, what each can suggest and where each one fails.
| Test | What it observes | What it can suggest | What it cannot decide |
| Pyrolysis | Chemical decomposition on heating, including volatile products and residue | Which decomposition family the polymer belongs to | Identity from one pyrolysis phenomenon, because temperature, atmosphere, residence time, sample form and additives all shift the result |
| Burning | Flame character, burning persistence, smoke, dripping and residue | A first guess at the polymer family | Anything dependable when flame retardants, pigments or fillers are present; the same polymer behaves differently after flame retardant modification and different polymers can look alike |
| Melting and softening | Softening and melting during controlled heating | Whether the material is semi-crystalline or amorphous, and roughly where it transitions | Fine separation, because melting ranges can overlap and blends can show several transitions |
Pyrolysis is about chemical decomposition. Given enough heat, chains can break, rearrange or react in other ways, producing different volatile products and residues, and polymers with different structures decompose differently. Burning is about what happens under flame: the flame’s character, whether it keeps burning, the smoke, the dripping and the residue all supply leads for a preliminary judgment. Melting is about softening and melting during heating, and for semi-crystalline thermoplastics it ties back to the crystalline structure, while amorphous plastics are better described through glass transition and softening.
Safety is not a footnote here. Unknown plastics can release harmful decomposition products as they heat. Do not judge a material by smelling the fumes, and do not burn unknown samples without local exhaust and appropriate protection. A burn test is not a flame reference table, and treating it as one is how false identifications get locked in early.
When accuracy matters, move to controlled thermal analysis. Differential scanning calorimetry characterizes melting, crystallization and related transitions, with ASTM D3418 covering how transition temperatures are determined. Thermogravimetric analysis goes after thermal decomposition and residual mass change. The two answer different questions and cannot substitute for one another.
Heteroatom tests: reading elements to shrink the candidate list
In polymer identification, a heteroatom is any element other than carbon and hydrogen: oxygen, nitrogen, sulfur, chlorine and fluorine among them. Polymers differ in elemental composition, and those differences are useful leads. Polyamides contain nitrogen and oxygen, polycarbonate contains oxygen, some chlorinated polymers contain chlorine, and fluoroplastics contain fluorine.
Table 5. Classical heteroatom routes, the polymer families they point toward and why the result is not decisive.
| Element sought | Classical detection route | Polymer families it suggests | Why the result is not decisive |
| Nitrogen | Sodium fusion followed by a nitrogen-specific color or precipitation reaction | Polyamides, polyurethanes, acrylonitrile copolymers such as ABS, aramids | Additives and fillers can contribute nitrogen, and many polymers share the element |
| Chlorine | Copper wire flame test, where a green flame indicates a halogen | PVC, chlorinated PVC, PVDC, chlorinated rubbers | A green flame does not separate PVC from another chlorinated resin |
| Sulfur | Lead acetate paper, which darkens in the presence of hydrogen sulfide | Polysulfones, polyphenylene sulfide, vulcanized rubbers | Sulfur-bearing additives produce false positives |
| Fluorine | Zirconium-alizarin lake, which loses its color when fluoride is present | PTFE, FEP, PFA, PVDF, ETFE, PCTFE, ECTFE | Cannot separate one fluoropolymer from another |
| Oxygen | Not detected by the classical element tests, so it is inferred from functional groups | PC, PET, POM, PMMA, polysulfones | Oxygen is present in most additives and fillers |
Element information is not a chemical identity. Detecting nitrogen does not make a sample a polyamide. Detecting chlorine does not confirm PVC. Detecting fluorine does not distinguish PTFE, FEP, PFA, PVDF or ETFE from one another. Different polymers can contain the same element, and pigments, fillers, flame retardants and other additives can introduce elements that the resin itself does not contain.
Heteroatom testing therefore belongs in the screening stage, where it cuts the candidate list. Confirming a specific polymer still requires infrared spectroscopy, thermal analysis or another suitable method. Any traditional test using special chemical reagents belongs in a laboratory equipped for it, and should not be simplified into a routine workshop step.
Classification analysis: narrow the range before naming the material
Suppose a batch of pellets of unknown origin arrives with low density and the appearance of an ordinary thermoplastic. PE and PP move to the front of the candidate list, and infrared spectroscopy, thermal behavior and other applicable tests decide between them. If the sample shows features associated with polyamides, the work shifts to PA and its relatives. If fluoropolymer features dominate, the question becomes which fluoropolymer.
Most plastic identification methods follow that staged pattern, eliminate first and confirm later. Every test should answer one defined question rather than adding to a pile of results.
Table 6. A generic classification framework. It is not a sequence every sample must complete.
| Stage | What you are deciding | Evidence that moves you on |
| 1. Problem definition and sampling | Which question the analysis must answer, and which object represents it | Sample identity, source and processing history |
| 2. Screening | Which broad family the material belongs to | Density band, heat response, element screen |
| 3. Structural confirmation | Which polymer it is | Infrared spectrum matched against references |
| 4. Composition | What else is present and at roughly what level | Thermal analysis, ash, elemental mapping |
| 5. Reporting | What is proven, what is supported and what remains open | Documented conditions and retained samples |
The framework is general on purpose. The actual test route should follow the sample, the analytical target and the evidence already in hand, not a fixed checklist completed in order.
Specific identification reactions and their three failure modes
Some traditional methods use a specific chemical reaction to produce a color change, a reaction product or another observable effect. They have historical value and they illustrate how polymer chemical analysis works, but three questions decide whether the result means anything.
- Selectivity. If several materials can produce a similar effect, the reaction is supporting evidence only and cannot carry the conclusion alone.
- Interference. Pigments, fillers, stabilizers and other additives can shift the color or change the course of the reaction.
- Control of conditions. Reagent state, reaction environment, sample preparation and observation conditions all affect the outcome.
A specific reaction belongs inside a complete analysis sequence, not at the front of it. A color appearing with a given reagent does not by itself assign the sample to a polymer. Any procedure that uses toxic, corrosive or otherwise hazardous reagents must run under a validated method with proper safety controls.
Where plastic identification goes wrong most often
For processors, the misjudgments that cost money happen between materials that are structurally close, visually similar, or modified. Five pairs account for most of them.
Table 7. Common confusions, the reason for the confusion and what actually separates the materials.
| Confusing pair | Why it confuses | What separates them |
| PE and PP | Density ranges can approach each other, especially in modified grades | FTIR plus thermal data; PP melts near 160 to 170 degrees Celsius against 105 to 135 degrees Celsius for PE |
| PA6 and PA66 | Identical functional group, so some infrared features look alike | Reference spectra combined with thermal analysis; a single feature peak is not enough |
| PC and ABS | Different structures, but PC/ABS alloys carry features of both | Judge an alloy as an alloy; forcing the sample into pure PC or pure ABS is the error |
| Unfilled resin and filled compound | Same polymer class, different density, ash and mechanical behavior | Identify the polymer first, then measure filler content as a separate finding |
| Fluoropolymers as one group | PTFE, FEP, PFA, PVDF, ETFE, PCTFE and ECTFE all resist chemicals and heat | Infrared spectroscopy and thermal analysis; color, corrosion resistance and temperature rating cannot separate them |
For quality disputes over high-performance materials, a screening result is not a final identification. Treating it as one is the expensive version of the same mistake.
FTIR: reading chemical bonds instead of appearances
Fourier transform infrared spectroscopy is one of the standard plastic identification methods. Chemical bonds absorb across specific wavenumber ranges, and different molecular structures produce spectra with characteristic features. Comparing absorption peaks against reference spectra shows whether the chemical structure agrees with a polymer class.
Table 8. Absorption features that carry most of the identification work.
| Absorption feature | Wavenumber (cm-1) | Typically associated with |
| O-H stretch | 3200 to 3600 | Alcohols, phenols, absorbed moisture |
| N-H stretch | 3300 to 3400 | Polyamides, polyurethanes, aramids |
| C-H stretch | 2850 to 2960 | All polyolefins and most organic polymers |
| Isocyanate N=C=O | 2270 | Uncured polyurethane systems |
| Carbonyl C=O stretch | 1700 to 1750 | PET near 1720, PMMA near 1730, PC near 1770 |
| Amide I and amide II | 1640 and 1540 | Polyamides and proteins |
| Aromatic C=C | 1450 to 1600 | PS, PC, PET, ABS |
| C-O-C stretch | 1000 to 1250 | PET, POM, PC, polysulfones |
| C-F stretch | 1000 to 1250, very strong | PTFE, FEP, PFA, PVDF |
| C-Cl stretch | 600 to 800 | PVC and chlorinated polymers |
Polymers carrying a carbonyl group show the corresponding carbonyl absorption, aromatic materials show aromatic ring features, and different fluoropolymers give spectra tied to their individual structures. Sample form decides the measurement mode. ATR-FTIR is the usual choice for fast surface screening of pellets, films, pipe and molded parts, while thin films can be run in transmission.
The limits deserve as much attention as the peaks. Surface oil, coatings or other contamination distort the spectrum. A blend shows features of several components at once, so a PC/ABS alloy produces a spectrum that is not simply the sum of two clean references. Two polymers with similar structures may not be separable by simple library matching. Infrared results should be read alongside the sample’s origin, thermal behavior and other evidence.
DSC and TGA: thermal evidence for material differences
DSC and TGA serve different purposes and are often confused because both involve a temperature program.
DSC studies the thermal effects a material shows as temperature changes: melting, crystallization and glass transition. For semi-crystalline plastics it characterizes melting behavior, and for some blends it reveals transitions tied to individual components. For amorphous plastics, the glass transition carries most of the information.
TGA follows mass change under a defined temperature program and atmosphere. It studies thermal decomposition behavior, changes in volatile content and the residual mass of filled materials. The common trap is reading that residue as filler content. Some polymers char rather than burning cleanly under the test conditions, and fillers themselves can lose or gain mass during the program.
Both techniques supply evidence for identification and composition analysis. Neither one closes an identity assignment on its own in every case.
SEM-EDS and XRF: when the question becomes what else is in there
When the question shifts from “which plastic is this” to “what else is present,” other methods come into play. Scanning electron microscopy shows micromorphology, and energy-dispersive X-ray spectroscopy reports the elemental composition of the region being examined. Together they suit filler distribution, particle shape and the elemental signature of an anomalous area. An unknown particle in a plastic can be imaged first, then screened by EDS for calcium, silicon or titanium. EDS reports elements only, so the presence of an element does not confirm a compound.
X-ray fluorescence screens many elements at once and has value in the analysis of some inorganic fillers and pigments, but it does not replace molecular structure analysis of the polymer.
Table 9. Matching the method to the stated analytical target.
| Analytical target | First-choice method | Why it fits | What it does not give you |
| Polymer identity | FTIR | Reports functional groups directly and matches reference spectra | Grade, molecular weight distribution, additive loading |
| Thermal transitions | DSC | Locates melting, crystallization and glass transition temperatures | Chemical structure |
| Decomposition and residual mass | TGA | Reports mass loss steps and residue | Filler content without method validation |
| Anomalous particle composition | SEM-EDS | Combines morphology with local element mapping | Compound identity from element presence alone |
| Inorganic filler or pigment elements | XRF | Rapid multi-element screen | Anything about the polymer backbone |
The order follows the question you are asking. Identify the polymer with FTIR when structure is what matters, reach for SEM-EDS when the problem is a stray particle, and turn to TGA, ash testing or other supporting methods when filler content is the issue.
Identifying historical and aged plastic objects
Plastic identification methods also apply to older objects, historical items and materials whose storage history is unknown, not only to modern production.
Early plastics differ from modern industrial grades. Formulations are undocumented, materials have aged, surfaces are contaminated and original technical data may not exist. Ageing shows up as yellowing, cracking, embrittlement or surface exudation, driven by structural change, additive loss and long environmental exposure. An aged appearance cannot be compared directly with the typical features of a new material of the same type.
For objects with conservation value, destructive sampling should be kept to a minimum, and non-destructive or micro-sampling methods should be assessed first. The conclusion then rests on chemical structure, physical features, sample condition, conservation history and intended purpose at the same time.
Building a plastic identification workflow a plant can use
For compounders, masterbatch producers, recyclers and processors, five steps cover most of the routine work. The sequence applies plastic identification methods in a deliberate order rather than as a fixed battery.
- Define the target. Confirm the main polymer, characterize an anomaly, identify a filler or contaminant, or verify a grade requirement. Different targets need different test plans.
- Collect sample information and take a defined sample. Record source, processing history, appearance and any known material data. Sample surface exudate, inclusions and bulk material separately instead of testing a mixture.
- Screen with simple tests. Appearance, density and applicable thermal tests establish the candidate range.
- Choose instruments against the question. FTIR, DSC, TGA, SEM-EDS or another suitable method, selected deliberately rather than applied to every sample as a fixed battery.
- Report with evidence and boundaries. Separate what is confirmed, what supports the judgment and what remains uncertain. For disputes, retain the original sample, the test conditions and the records so the result can be reviewed.
Naming needs discipline too, so the plant should standardize abbreviations. ISO 1043-1 sets out the abbreviations and symbols used for base polymers and their special characteristics, which reduces confusion in material naming and symbol misuse.
A resin identification code on a product is not a quality certificate. ASTM D7611/D7611M covers how resin identification codes are used and makes clear that the code is not a recycling code and does not by itself prove that an item can be effectively recycled.
What these methods cannot prove
The most useful thing to understand about plastic identification methods is where each one runs out. That boundary separates a defensible conclusion from a guess, well before any catalog of observed phenomena does.
- Density narrows the candidate range and may not separate structurally similar materials.
- A burn test supplies supporting information and is easily dominated by additives and test conditions.
- FTIR identifies polymer structure and does not establish a specific grade.
- Element analysis finds which elements are present and cannot say what chemical form they take.
- A heteroatom result places a sample in a family and, alone, cannot separate PVC from another chlorinated resin, or PTFE from FEP.
- TGA residue is an upper bound, not a filler content.
So the same nominal polymer can be described with very different confidence. Saying that a spectrum matches PP is a different claim from saying the material is a PP homopolymer with a stated melt flow rate and a stated filler level. Both can be correct, and a report that does not distinguish them invites the reader to assume more than the evidence supports.
Practical recommendations
- Start with density. It costs minutes, requires almost no equipment and eliminates whole families before any instrument time is booked.
- Do not decide a polymer from a flame color alone. Use burning as a screening signal and confirm with FTIR.
- Run FTIR before thermal analysis when structure is the question, and reserve DSC and TGA for the cases where transitions or decomposition actually matter.
- Read the meaning of a TGA residue before converting a curve into a filler percentage.
- Sample the anomaly, not the part. An exudate or a stray particle deserves its own analysis even when the surrounding material is known.
- Retain the original sample, the test conditions and the records whenever the result could become a dispute.
- Keep reagent-based classical tests in a laboratory with the containment, waste handling and validated method they need.
- State the uncertainty in the report rather than letting the reader infer more confidence than the evidence carries.
Limitations
- The density and melting ranges in this article are typical values for unfilled polymers taken from public material data. They are screening windows and not grade specifications, and filled or modified grades will sit outside them.
- This article describes method logic and method capability. It is not a validated in-house procedure and does not replace the applicable test standard or the supplier datasheet.
- Additives, blends, fillers, processing history and moisture change measured values. Polyamide density shifts with moisture content, and thermal transitions shift with thermal history.
- Instrument availability differs widely between plants. A laboratory without FTIR can still narrow a candidate list, but it cannot confirm a polymer structure, and the report should say so rather than imply confirmation.
- Standards and regulatory frameworks are revised over time. Confirm the current edition before quoting any standard in a test plan.
- Some traditional heteroatom and specific-reaction tests use hazardous reagents. They belong in a laboratory with the appropriate controls, not on a production floor.
- The plastic identification methods described here follow standard laboratory practice, but any plant method has to be validated against its own reference materials before results are used for a release decision.
- The polymer abbreviations used here follow common industry practice. Where a formal abbreviation matters, use the current standard rather than informal usage.
Bottom line
Plastic identification methods form a chain of evidence rather than a lookup table. Screening tests cut the candidate list cheaply, FTIR names the polymer, and thermal and elemental methods describe what else is present. Each link proves something narrower than people assume, and the report that says which link supports which claim is the one that holds up under review.
FAQ
What does a density test tell you about an unknown plastic
A density reading narrows the candidate list before any instrument work begins. Unfilled polyolefins sit at 0.89 to 0.96 g/mL and float in water, while most engineering polymers sit above 1.04 g/mL and sink. It cannot separate materials with overlapping ranges, and fillers or foaming shift the value well away from the base resin.
Can a burn test identify an unknown plastic on its own
No. Flame character, smoke and drip behavior are shaped by flame retardants, pigments and fillers as much as by the base resin. Treat a burn test as a screening signal that points toward a family rather than as a final identification, and remember that it releases decomposition products which should not be inhaled.
Why is ATR-FTIR the usual first choice for polymer identification
ATR-FTIR reads the surface of a solid sample in seconds with little preparation and produces a spectrum that can be matched against reference libraries. It identifies the functional groups that separate most commodity polymers, including carbonyl, amide, aromatic and carbon and fluorine features. Heavily filled, coated or degraded surfaces and blends remain difficult.
What is the difference between DSC and TGA in plastics analysis
DSC measures heat flow and locates melting, crystallization and glass transition temperatures. TGA measures mass loss against a temperature program and reveals decomposition steps, volatile content and residue. Run both when a melting point alone is ambiguous, because they answer different questions and neither one covers the other.
How do you tell PE and PP apart
Density ranges often overlap, so combine infrared data with thermal data. PP melts near 160 to 170 degrees Celsius while polyethylene melts between 105 and 135 degrees Celsius, a gap wide enough to separate the two in a single DSC run. Infrared adds a methyl feature near 1375 cm-1 that polyethylene does not show.
How do you tell PA6 and PA66 apart
Both show amide absorption, so no single peak separates them. Their melting points differ, with PA6 near 220 degrees Celsius and PA66 near 255 to 265 degrees Celsius, which is the most practical split for a routine laboratory. Compare the full spectrum against reference standards rather than relying on one feature peak.
Can FTIR confirm a specific plastic grade
No. FTIR establishes the polymer class and can flag major additives such as fillers or plasticizers. Melt flow rate, molecular weight distribution and additive loading differ between grades of the same polymer and stay invisible in an infrared spectrum. A grade claim needs supplier documentation plus physical and mechanical testing.
What does a heteroatom test actually detect
Most plastic identification methods use heteroatom testing to establish which elements other than carbon and hydrogen are present, including nitrogen, chlorine, sulfur and fluorine. A positive result places a sample in a broad family and does not settle the polymer, because additives and fillers introduce the same elements. Use it to cut the candidate list before infrared work.
How do you test a filled or glass fiber reinforced plastic
Identify the polymer first with FTIR and treat filler content as a separate measurement. Ash testing after combustion or TGA in air gives an approximate inorganic fraction that can be cross-checked against the thermogravimetric curve. Report polymer and filler as two findings, because different methods produced them.
Why does TGA residue not equal filler content
Some polymers char instead of burning cleanly, and that char mass is then counted as residue. Fillers themselves can release water or decompose within the temperature program, so the final mass is not a clean inorganic fraction. Treat the residue as an upper bound unless the method has been validated against known formulations.
Do resin identification codes tell you what a plastic is made of
A resin identification code names the base resin family for sorting purposes and is not a composition or quality certificate. The code does not prove recyclability and says nothing about additives, fillers or grade, so it cannot support a purchasing or warranty decision. Verify identity by analysis whenever the outcome depends on it.
How should a plant sample an unknown contaminant
Sample the contaminant separately from the bulk material even when the two appear related. Keep the original sample, the sampling location and the processing history attached to the test request. Surface deposits can originate from the polymer, from an additive, from an external contaminant or from equipment residue, and each of those routes implies a different corrective action.