PTFE Friction Testing: Why That Single Number Is Probably Wrong

Why a Single Friction Coefficient Tells You Almost Nothing

Ask most engineers what makes PTFE special, and they will say “low friction.” They are not wrong, but they are oversimplifying. The friction coefficient of PTFE is not a material property you can look up in a table and call it a day. It depends on the form of PTFE you are using (pure resin, filled compound, thin film, coating, or bearing liner), what it is sliding against, how smooth that surface is, how hard it is, how much load is applied, how fast things are moving, what the temperature is, whether there is lubrication, and whether the system has had time to break in.

ASTM G99 puts it plainly: wear and friction results depend on load, speed, sliding distance, environment, material properties, and machine characteristics. If you test under conditions different from the standard, document those differences. The result cannot be equated to standard interlaboratory study results.

When calculating friction coefficient, static friction comes from the peak force before movement starts. Dynamic friction is the average value during steady sliding. Do not mix running-in data, stick-slip peaks, and steady-state values together.

Reference Data from Major Brands

Here are typical friction ranges from major PTFE suppliers. Useful for setting test targets and acceptance windows, but do not rank them directly across different test methods. They were not generated the same way.

Chemours Teflon PTFE Resin — Dynamic friction 0.05–0.10 per ASTM D1894. Good as a QC baseline for pure PTFE resin sheets and films.

Chemours Teflon Industrial PTFE Coatings — Static friction around 0.12–0.15, dynamic around 0.05–0.10. The same data sheet says low friction depends on load, speed, and the specific coating system. Coating evaluation needs to look at friction together with adhesion, thickness, and cure state.

Daikin POLYFLON PTFE Coatings — TC-7409BK: 0.04–0.08. TD-7139BD: 0.04–0.07. Tested with Bowden-Leben method, 8 mm steel ball, 0.27 cm/s, 1.0 kg load. Daikin says these are typical values, not guarantees.

SKF PTFE Composite Plain Bearings — 0.03–0.25. SKF says friction depends on load, speed, temperature, surface roughness, contamination, and lubrication. Higher loads and lower speeds generally give lower friction. Friction may increase above 100°C.

GGB DU-B PTFE Plain Bearings — Dry: 0.02–0.25. Oil-lubricated: 0.02–0.12. The data sheet clearly shows how lubrication shifts the friction window and allows higher sliding speeds and pV values.

Omniseal / Saint-Gobain Rulon LR — 0.15–0.25, PV 0.35 MPa·m/s. Rulon LR is a ceramic-filled PTFE-grade. Higher friction than pure PTFE, but better wear resistance and creep stability.

Saint-Gobain Rulon Material Family — Friction decreases as load increases. Harder counterfaces lead to lower wear. PTFE-based materials wear more in steam and wet environments than in dry conditions. Counterface material and wet environments must be included in the test matrix.

Choosing the Right Test Standard

Thin films, sheets, and surface slip QC

Use ASTM D1894 or ISO 8295. These standards measure static and sliding friction of plastic film and sheeting sliding over itself or other materials. One catch: ASTM says D1894 and ISO 8295 are not equivalent, and results cannot be directly compared.

The procedure goes like this: condition the specimen for temperature and humidity, confirm orientation and thickness, mount the PTFE specimen or counterface, apply the specified sled and load, pull at the specified speed, record starting peak and sliding forces, and calculate static and dynamic coefficients. Repeat for each direction and surface.

These methods work for PTFE film, skived tape, laminated surfaces, and low-friction surface QC.

One thing ASTM D1894 flags: friction of plastic films and sheets is sensitive to speed, surface condition, sample aging, processing history, loading rate, and dwell time before testing. Batch comparisons need to control sample timing, surface cleaning, dwell time, and speed.

Dry sliding, wear, and engineering tribosystems

Use ASTM G99 (pin-on-disk or ball-on-disk), ASTM G133 (reciprocating ball-on-flat), ASTM D3702 (thrust washer), or ISO 7148-2 (polymer bearing materials).

ASTM G99 covers sliding friction and wear testing for pin-on-disk and ball-on-disk. The standard itself says it does not reproduce actual service conditions for lubrication, load, pressure, contact geometry, debris removal, or corrosive environments. Read that carefully.

ASTM G133 works for reciprocating linear sliding. It measures wear volume and dynamic friction coefficient, with both non-lubricated and lubricated procedures.

ASTM D3702 measures wear rate and friction coefficient of self-lubricating materials in a thrust washer setup. Test below the material PV limit.

ISO 7148-2 covers tribological testing of polymer-based bearing materials under specified load, sliding speed, temperature, with or without lubrication.

Detailed Test Protocols

A. Static Friction Coefficient

Static friction testing evaluates PTFE resistance at startup, stop-start motions, low-speed positioning, seal lip breakaway, and initial movement on guide rails. PTFE static friction is typically low, but the startup peak can change significantly after prolonged load dwell, temperature rise, surface contamination, or lubricant drying.

For film and sheet QC, use ASTM D1894 or ISO 8295. For engineering tribosystems, ASTM G219 offers an inclined plane method for startup friction screening. For bearing and seal applications, do breakaway testing with actual counterface material after load dwell.

The procedure: clean and dry the specimen and counterface. Record counterface material grade, hardness, surface roughness Ra/Rz, and surface treatment. Apply the target normal load. Set dwell time (try 0 min, 10 min, 1 h, 24 h) to simulate real stop states. Start sliding at the specified loading rate or incline angle speed. Record the maximum tangential force before movement. Calculate static friction coefficient.

Here is where it gets interesting. Static friction is highly sensitive to loading rate and dwell time before startup. ASTM D1894 specifically flags this. PTFE undergoes cold flow and micro-conformation, so the startup peak can rise after prolonged load dwell. Products like seals, guide rails, bridge bearings, and sliding bearings need a dedicated breakaway test after stop periods, not just continuous sliding friction data.

B. Dynamic Friction Coefficient

This one evaluates steady-state friction of PTFE during continuous sliding. Relevant for bushings, guide rails, sliders, seals, coatings, and wear liners.

For sheets and films, ASTM D1894 or ISO 8295. For point or line contact, ASTM G99 or ASTM G133. For bearing materials, ASTM D3702 or ISO 7148-2.

The procedure: set normal load, speed, temperature, and sliding distance. Start sliding and record the friction-time curve continuously. Identify three phases: startup peak, running-in, and steady state. Calculate average dynamic friction coefficient from the steady-state region. Also record maximum, minimum, standard deviation, stick-slip amplitude, and surface temperature rise. After testing, examine the wear track, transfer film, debris, and counterface condition.

A practical tip: PTFE forms a transfer film during dry sliding. SKF notes that PTFE composite bearings go through a running-in phase where PTFE transfers to the counterface. Only after this transfer is complete does the material show its low friction and low wear. Report the data window clearly. For example, exclude the first 500 m of running-in and take the steady-state average from 500 to 2000 m. If you only take the first few dozen seconds, the result will be higher and more erratic.

C. Dry Friction

PTFE core advantage is self-lubrication, so dry friction testing is the most fundamental test. Relevant for oil-free bearings, clean environments, food equipment, medical and bioprocess equipment, semiconductor equipment, vacuum, and low-contamination applications.

Use ASTM G99, ASTM G133, ASTM D3702, or ISO 7148-2.

The procedure: clean the specimen and counterface with specified solvents and dry completely. Do not touch sliding surfaces with bare hands. Measure initial roughness, hardness, thickness, and mass. Set dry environment conditions: temperature, humidity, air/nitrogen/vacuum. Set load, speed, and distance or time. Continuously record friction force and near-contact temperature. After testing, record wear track width, wear volume, and counterface transfer film.

One thing people get wrong: dry friction is not “no controls.” Environmental humidity, air composition, debris removal, and whether the sample was pre-run-in all need to be documented. Pure PTFE may have lower friction but does not necessarily have the best wear resistance or creep resistance. Filled PTFE grades often have slightly higher friction but significantly better load-bearing capacity, wear resistance, and dimensional stability. Rulon LR, for example, has a friction coefficient of 0.15 to 0.25, but it is positioned as a high-creep-resistance bearing-grade filled PTFE.

D. Lubricated Friction

This test evaluates how oil, grease, water, process fluids, or boundary lubrication affect PTFE friction, wear, transfer film formation, and failure mode.

Use ASTM G133 or ISO 7148-2. For bearing products, use thrust washer, bushing, or actual component bench testing.

The procedure: select the lubricant (mineral oil, synthetic oil, PFPE, silicone oil, grease, water, process fluid). Record lubricant viscosity, temperature, additives, delivery method, and film condition. Define lubrication mode: single application, drip feed, oil bath, circulation, grease. Set speed and load to place the contact in boundary, mixed, or hydrodynamic regime. Record friction coefficient changes over time and temperature. After testing, check whether the transfer film has been weakened or washed away by the lubricant.

The data can be surprising. Lubrication generally reduces friction. GGB DU-B data shows dry friction 0.02 to 0.25 versus oil-lubricated 0.02 to 0.12, with higher allowable speeds and pV values under oil. But lubrication does not automatically reduce wear. PTFE relies on transfer film to build a low-friction interface. Some lubricants, water, or steam environments can disrupt transfer film formation. Omniseal notes that PTFE-based materials wear more in steam and wet environments than in dry conditions.

Do not report just a lubricated friction coefficient. Include the lubricant name, viscosity grade, additives, supply rate, temperature, contamination control, and post-test oil condition. Lubricants containing solid contaminants can cause abrasive wear on PTFE surfaces, raising both friction and wear.

E. Counterface Material Effects

This one determines friction and wear differences when PTFE pairs with different metals, ceramics, glass, plastics, or coatings.

Common counterface materials include 304 and 316 stainless steel, hardened bearing steel or tool steel, hard chrome, nickel plating, DLC, anodized aluminum, brass, bronze, aluminum alloy, ceramic balls, glass, POM, PEEK, and PTFE itself.

The procedure: keep the PTFE material constant and change only the counterface. For each counterface, use a uniform roughness grade (Ra 0.05, 0.2, 0.4 µm, for example). Measure hardness, roughness, surface energy, or contact angle. Run both dry and lubricated comparisons at the same load, speed, and temperature. After testing, observe counterface transfer film continuity, scoring, adhesion, and debris. Evaluate using both wear rate and friction coefficient, not friction alone.

Harder, more stable counterfaces generally reduce wear. Omniseal notes that Rulon material wear decreases as counterface hardness increases. SKF recommends soft carbon steel ground surfaces for PTFE composite bearings, with Ra not exceeding 0.4 µm. For more demanding conditions, hardened counterfaces with at least 50 HRC and Ra no greater than 0.3 µm are recommended. GGB DU-B data sheets also provide shaft surface roughness and hardness recommendations, confirming that counterface condition is a key input to bearing friction testing.

F. Load, Speed, and Temperature Effects

Load. PTFE and filled PTFE friction coefficients often decrease as load increases. But higher loads bring creep, contact temperature rise, transfer film disruption, and PV limit risks. Omniseal explicitly states Rulon friction decreases with increasing load.

Set low, medium, and high load levels. Express in contact pressure, not just mass. Keep speed and temperature constant across load levels. Record friction curve, temperature rise, wear rate, and permanent deformation. Calculate PV before high-load testing.

Speed. Higher speed changes shear heating, transfer film formation, lubrication regime, and stick-slip behavior. Chemours notes Teflon coating friction depends on load, speed, and the specific coating system. SKF also identifies load, sliding speed, and temperature as the main factors determining composite bearing friction.

Set low, medium, and high speeds based on the application range. Keep load and temperature constant. Run each speed to steady state. Record temperature rise. At high speeds, frictional heat can mask intrinsic material differences. For stop-start applications, add low-speed reciprocating and stick-slip testing.

Temperature. PTFE operates across a wide temperature range, but friction, creep, crystallinity, hardness, and transfer film all change with temperature. SKF notes PTFE composite bearing friction increases above 100°C. Chemours Teflon coatings can be used continuously to around 260°C, but friction still depends on operating conditions.

Use 23°C as room temperature baseline. Low temperature per application (try -40°C, -80°C or lower). High temperature per material and application (80°C, 120°C, 150°C, 200°C). Let specimen and counterface reach thermal equilibrium before starting. Measure temperature near the contact zone, not just the chamber temperature. For high-temperature lubricated tests, record lubricant viscosity change and oxidation or volatilization state.

Recommended Test Matrices

Basic QC Matrix

  • Specimen: Same batch PTFE sheet, film, or coating, minimum 3 pieces
  • Counterface: Polished stainless steel or specified engineering counterface
  • Temperature: 23°C
  • Condition: Dry
  • Output: μs, μk, friction curve, mean, standard deviation
  • Method: ASTM D1894, ISO 8295, or simplified sled method

Engineering Validation Matrix

  • Counterface: Stainless steel, hardened steel, aluminum alloy or anodized aluminum, actual shaft material
  • Roughness: Ra 0.05, 0.2, 0.4 µm, or as per actual part
  • Load: Low, medium, and high, converted to contact pressure
  • Speed: Low-speed start-stop, medium continuous, high-speed limit
  • Temperature: 23°C, application high temperature, application low temperature
  • Lubrication: Dry, oil, grease, water or process fluid
  • Output: Breakaway friction, steady-state friction, temperature rise, wear rate, transfer film, counterface damage

Bearing or Sliding Component Matrix

  • Method: ASTM D3702, ISO 7148-2, or actual bushing bench test
  • Core parameters: p, v, temperature, lubrication state
  • Criteria: Friction coefficient plus wear rate plus dimensional change plus failure mode
  • Key constraint: Do not exceed the material PV limit. D3702 emphasizes testing below the PV limit.

Key Takeaways

PTFE friction testing is not a one-number exercise. The friction coefficient changes with every variable in the system. A proper test report includes the PTFE form, counterface material and roughness, load, speed, temperature, lubrication, running-in state, test standard, and data extraction method. Static and dynamic friction must be treated separately. Running-in and steady-state values must not be mixed. Counterface hardness and roughness must be documented. Lubrication changes the friction window but does not guarantee lower wear. And temperature, especially above 100°C, can fundamentally alter PTFE tribological behavior.

Design meaningful test matrices, not single-point measurements. The difference between 0.05 and 0.25 is not material variation. It is the difference between testing film on polished steel at low load and testing a filled bearing liner against a rough shaft in a hot environment. Both numbers are real. The question is which one matches your application.