PU rigid foam raw materials decide insulation performance, fire rating, and cost. This handbook walks through 50 key ingredients across seven families: polyols, isocyanates, catalysts, blowing agents, surfactants, flame retardants, and fillers. Each entry gives hydroxyl value, functionality, NCO content, or blowing agent class where it matters, plus typical use. Four selection rules close the piece.
Rigid polyurethane foam has the lowest thermal conductivity of any organic insulation material. It is the backbone of polyurethane insulation in construction, cold chain, pipe insulation, and water heaters. One formula means many moving parts: change the polyol and you change strength and dimensional stability; change the blowing agent and you change lambda value and environmental class; change the flame retardant and you change the fire rating. Selecting PU rigid foam raw materials starts with the application.
The tables below list the key raw materials in seven groups, copied from the source handbook. Hydroxyl value is in mgKOH/g. Functionality is the average number of reactive sites per molecule. NCO is the isocyanate group content. ODP and GWP mark the environmental profile of blowing agents.
PU Rigid Foam Raw Materials: The Seven Component Families
Each rigid foam formula sits on seven pillars. The table gives the role of each family and its typical place in the recipe.
| Component family | What it decides | Typical place in recipe |
| Polyols | Strength, dimensional stability, and the thermal conductivity floor | Main resin; polyol count is 100 parts |
| Isocyanates | Crosslink density, reaction speed, and heat resistance | Black material; dose indexed to polyol |
| Catalysts | Gel-blow balance, cure speed, and demold time | Small dose, about 0.1 to 3 parts |
| Blowing agents | Cell structure, lambda value, and environmental class | Physical agent or chemical water |
| Surfactants | Cell size, cell opening, and surface defects | 1 to 2 percent |
| Flame retardants | Fire rating such as B1, and smoke suppression | Additive or reactive type |
| Fillers and release agents | Compression strength, cost, and demold integrity | Optional |
Polyols: The Backbone That Sets Strength and Dimensional Stability
Polyols set strength, dimensional stability, and the lower limit of thermal conductivity. The source lists twelve named polyols below.
| # | Polyol | Hydroxyl value | Functionality | Typical use |
| 01 | 4110 type sucrose-based polyether polyol | About 430 mgKOH/g | About 4.1 | General rigid foam backbone; boards, refrigerators, pipe insulation |
| 02 | 1056 type glycerol polyether polyol | About 560 mgKOH/g | 3 | All-water systems; spray rigid foam; low cost, fine cells |
| 03 | 835 type sucrose-sorbitol composite polyether | About 350 mgKOH/g | About 5 to 6 | High dimensional stability rigid foam; structural board, cold chain |
| 04 | 635 type low-hydroxyl-value glycerol polyether | About 350 mgKOH/g | 3 | Viscosity reduction and flow adjustment; blended with 4110 and 835 |
| 05 | 435 type medium-hydroxyl-value general polyether | 350 to 450 mgKOH/g | 3 to 4 | General rigid foam; ordinary insulation and filling foam |
| 06 | Pentaerythritol-based polyether polyol | 4 | High strength structural foam; imitation wood, structural parts, high-density foam | |
| 07 | Sorbitol-based polyether polyol | About 6 | High closed-cell rigid foam; refrigerators and freezers; renewable sugar alcohol starter | |
| 08 | Aromatic polyester polyol | 250 to 350 mgKOH/g | Flame resistance and dimensional stability; PIR board component; blended with polyether to cut cost | |
| 09 | Adipic acid-based polyester polyol | Adjustable range | Special rigid foam and RIM; strong substrate adhesion | |
| 10 | Phosphorus-containing flame-retardant polyether polyol | Phosphorus about 6 to 10 percent | Permanent flame retardance without migration; with TCPP cuts additive dose; B1 building insulation | |
| 11 | Grafted polyether polyol (POP) | Solids 20 to 45 percent | Reinforcement; cell opening stability | |
| 12 | PIR system polyol | For high isocyanate index 200 to 400; stable exotherm with excess pMDI; heat resistance 140 degrees Celsius and above |
Sucrose-based and sorbitol-based polyols carry high functionality and build dense networks for structural board. Glycerol-based polyols flow better and fit all-water and spray systems. Aromatic polyester polyols bring flame resistance and lower cost, often blended with polyether in PIR board. Reactive phosphorus polyols bond phosphorus into the chain for permanent flame retardance without migration.
Isocyanates: The MDI Side That Builds Crosslinks
Rigid foam almost always uses MDI-series black material. The isocyanate index decides the system type.
| # | Isocyanate | NCO content | Functionality | Typical use |
| 17 | Polymeric MDI (pMDI) | About 30 to 32 percent | 2.7 to 3.0 | Largest isocyanate use; lower vapor pressure than TDI; refrigerators, boards, spray |
| 18 | High-functionality polymeric MDI | 3.0 to 3.3 | Rigid foam reinforcement; continuous board lines; low-temperature construction | |
| 19 | Liquefied modified MDI | Carbamate or carbodiimide modified; liquid at room temperature; cast rigid and semi-rigid foam | ||
| 20 | MDI prepolymer | 18 to 25 percent | Low free MDI; adjustable viscosity; high environmental requirement occasions; low fogging value | |
| 21 | Isocyanurate-modified pMDI | Pre-built isocyanurate rings; PIR board; better heat resistance and flame retardance |
pMDI is the most used isocyanate in rigid foam. Its vapor pressure is far below TDI, so it is safer to handle. High-functionality pMDI cures faster and suits continuous board lines. Liquid modified MDI eases handling of cast systems. MDI prepolymers cut free monomer and fogging. Isocyanurate-modified pMDI is the base of PIR board, with isocyanurate rings pre-built for better heat resistance and flame retardance.
Catalysts: Balancing Gel, Blow, and Trimerization
Hard foam catalysis balances three reactions: gel, blow, and trimerization.
| # | Catalyst | Type | Main role | Typical use |
| 22 | Triethylenediamine (A-33) | Tertiary amine; 33 percent in dipropylene glycol | Gel plus blow balance | Classic workhorse; almost all rigid foam systems |
| 23 | Dimethylcyclohexylamine (DMCHA) | Cycloaliphatic tertiary amine | Gel-leaning | Main gel catalyst; boards and refrigerators; paired with A-33 |
| 24 | Pentamethyldiethylenetriamine (PMDETA) | Tertiary amine | Strong gel | High activity, low dose; low temperature and fast demold |
| 25 | N,N-dimethylbenzylamine | Tertiary amine | Gel-leaning, low cost | Traditional cost-effective catalyst; watch odor and VOC |
| 26 | Dimethylethanolamine (DMEA) | Hydroxyl-containing tertiary amine | Blow-leaning | Improves cell opening and flow; low-to-mid grade formulas |
| 27 | Triethanolamine | Alkanolamine | Post-cure and low-temperature catalysis | Helps foam mature and set; flattens reaction curve with strong amines |
| 28 | Dibutyltin dilaurate (T-12) | Organotin | Strong gel | Extreme gel efficiency at tiny dose; organic tin regulation trend |
| 29 | Potassium octoate or potassium isooctanoate | Alkali metal salt | Trimerization catalyst | PIR core catalyst; dose tied to isocyanate index |
| 30 | Quaternary ammonium trimerization catalyst | Quaternary salt; Dabco TMR series | Trimerization catalyst | More controllable than potassium salts; longer milk-white stage; high-end PIR |
TEDA A-33 is the classic workhorse, promoting both gel and blow. DMCHA and PMDETA lean toward gel and suit fast demold. DMEA leans toward blow and opens cells. Triethanolamine gives mild late-stage catalysis that flattens the reaction curve. T-12 organotin delivers extreme gel efficiency at tiny doses, though organic tin faces regulation pressure. Potassium salts and quaternary ammonium salts drive trimerization in PIR systems; quaternary salts allow a longer milk-white stage for better mold filling.
Blowing Agents: From HCFC-141b to HFO-1233zd(E)
Blowing agents decide lambda value and environmental grade. The industry is in the fourth-generation transition.
| # | Blowing agent | Type | Environmental mark | Typical use |
| 31 | HCFC-141b | Hydrochlorofluorocarbon | ODP above 0; phaseout transition | Existing equipment transition; new projects should choose alternatives |
| 32 | Cyclopentane | Hydrocarbon | ODP 0; GWP about 11 | Refrigerator and freezer mainstream; explosion-proof design needed |
| 33 | n-Pentane or isopentane | Hydrocarbon | Lower boiling point; higher foaming efficiency | Blended with cyclopentane; boards and spray |
| 34 | HFC-245fa | Hydrofluorocarbon | ODP 0; GWP about 1030 | Third-generation agent; non-flammable; being replaced by HFO |
| 35 | HFC-365mfc | Hydrofluorocarbon | Often blended with HFC-227ea for flame retardance | Europe market; GWP phase-down pressure |
| 36 | HFO-1233zd(E) | Hydrofluorolefin fourth generation | GWP about 1; non-flammable | Near-zero GWP; refrigeration and high-end building materials |
| 37 | Water | Chemical blowing with CO2 | Zero ODP and GWP; lowest cost | High lambda and embrittlement risk; usually blended in semi-water systems |
Cyclopentane is the mainstream agent for refrigerators and freezers, with mature equipment but flammability that needs explosion-proof design. n-Pentane and isopentane boil lower and foam more efficiently, often blended with cyclopentane. HFC-245fa and HFC-365mfc are third-generation agents being replaced by HFO because of high GWP. HFO-1233zd(E) is near-zero GWP, non-flammable, and already scaled in refrigeration and high-end building materials. Water gives zero ODP and GWP at the lowest cost, but CO2 conducts heat well and embrittles foam, so it is usually blended with a physical agent in semi-water systems.
New PU rigid foam raw materials designs should start from pentane or HFO to avoid forced reformulation after HCFC-141b phaseout.
Surfactants: The One to Two Percent Additive That Decides Cell Quality
Surfactants are polyether-modified organosilicones used at 1 to 2 percent, yet they decide cell quality.
| # | Surfactant | Feature | Typical use |
| 38 | General rigid foam polyether-modified silicone | Organosilicone surfactant; for example AK8805 type | Emulsifies blowing agent, stabilizes cells, cuts surface tension across most systems |
| 39 | Full-water system silicone | Water resistance; CO2 emulsification | All-water spray formulas; helps CO2 nucleate evenly, prevents coarse cells and collapse |
| 40 | Spray rigid foam silicone | Low-temperature flow plus fast cure | Balances substrate wetting and cell stability; prevents sagging and pinholes in winter |
| 41 | PIR high closed-cell silicone | High index tolerance; high heat tolerance | Survives high isocyanate index and high exotherm without brittleness |
| 42 | High-stability board silicone | Wide process window | Continuous board line high-speed production; fewer scrap boards |
General silicone emulsifies the blowing agent, stabilizes cells, and cuts surface tension across most systems. Full-water silicone helps CO2 nucleate evenly and prevents coarse cells and collapse in all-water spray formulas. Spray silicone balances substrate wetting and cell stability, preventing sag and pinholes in winter. PIR silicone survives high isocyanate index and high exotherm without brittleness. Board silicone gives a wide process window for continuous lines.
Flame Retardants: Additive and Reactive Phosphorus Systems
Building insulation makes flame retardants the third-largest rigid foam component.
| # | Flame retardant | Type | Phosphorus content | Typical use |
| 43 | Tris(2-chloro-1-methylethyl) phosphate (TCPP) | Additive halogenated phosphate | About 9.5 percent | Largest flame retardant use; B1 formulas typically 8 to 15 percent |
| 44 | Triethyl phosphate (TEP) | Additive phosphate; halogen-free | Halogen-banned scenarios; mild odor; higher volatility | |
| 45 | Dimethyl methylphosphonate (DMMP) | Phosphonate | About 25 percent | High efficiency, lower total dose; doubles as viscosity reducer; watch volatility |
| 46 | Diethyl hypophosphite (DEEP type) | Hypophosphite ester | Good hydrolysis resistance; high-end and export products; higher cost than TCPP | |
| 47 | Melamine | Nitrogen type; sublimation endothermic plus charring | P-N synergism with phosphorus; good smoke suppression | |
| 48 | Expandable graphite (EG) | Physical intumescent; 80 to 300 mesh common | Insulating char layer when heated; DIN 4102 B1 route; 8 to 15 percent |
TCPP is the most used additive flame retardant, with low viscosity and good polyol compatibility. B1 grade formulas typically use 8 to 15 percent TCPP, but halogen controversy and migration are concerns. TEP is halogen-free with mild odor but higher volatility. DMMP packs about 25 percent phosphorus for high efficiency and lower total dose, though it also volatilizes. DEEP hypophosphite esters resist hydrolysis better and suit high-end and export products at higher cost. Melamine gives P-N synergism with phosphorus and good smoke suppression. Expandable graphite forms an insulating char layer when heated and is a main route to grades such as DIN 4102 B1.
Mainstream cost-performance practice pairs an additive flame retardant with a reactive phosphorus polyol. Piling only TCPP will not reach high fire ratings.
Fillers and Mold Release Agents
| # | Additive | Type | Addition level | Typical use |
| 49 | Glass fiber or wollastonite reinforcement filler | Inorganic fiber filler | 5 to 20 percent | Structural board and imitation wood; raises compression strength and dimensional stability; raises viscosity and equipment wear |
| 50 | Rigid foam mold release agent | Silicone, wax, or water emulsion | Molded foam such as refrigerator liners, imitation wood, and pipe shells; decides demold integrity, surface quality, and topcoat adhesion; water-based is the green trend |
Glass fiber and wollastonite raise compression strength and dimensional stability while cutting thermal expansion, at the cost of higher viscosity and equipment wear. Mold release agents are a must for molded rigid foam such as refrigerator liners, imitation wood, and pipe shells; they decide demold integrity, surface quality, and topcoat adhesion.
Limitations
The source handbook introduces this section as 50 materials across seven families but names 46 items in the tables; treat the count as approximate. Blowing agent rules reflect phase-down schedules such as the Kigali Amendment and may differ by region. Hydroxyl values, functionality, NCO content, ODP, and GWP are typical ranges from the handbook, not product specifications; confirm with supplier datasheets before scaling.
Bottom Line
PU rigid foam raw materials work as a system, not a shopping list. Pick the polyol for the mechanics you need, the MDI grade for cure speed, the blowing agent for lambda and environmental rules, and the flame retardant for fire rating. Match PU rigid foam raw materials to the application, and validate with full fire test reports before you scale.
FAQ
What are PU rigid foam raw materials
They are the seven ingredient families that make a rigid polyurethane foam formula: polyols, isocyanates, catalysts, blowing agents, surfactants, flame retardants, and fillers or release agents. Polyols build the polymer backbone, isocyanates crosslink it, and blowing agents open the cells. Catalysts tune the reaction speed, surfactants shape the cells, flame retardants set the fire rating, and fillers or release agents add strength or ease demolding. The choice of each family moves insulation performance, fire safety, and cost at the same time.
Which polyol is the default backbone for rigid foam
The 4110 type sucrose-based polyether polyol is the default base stock in many board, refrigerator, and pipe insulation formulas. It has a hydroxyl value of about 430 mgKOH/g and functionality of about 4.1, giving high crosslink density and balanced strength with dimensional stability. Glycerol-based polyols such as 1056 suit all-water and spray systems instead. Choose sorbitol-based or sucrose-sorbitol polyols when high dimensional stability and compression strength matter most.
Why does rigid foam use pMDI instead of TDI
Rigid foam almost always uses MDI-series black material because pMDI vapor pressure is far below TDI, which makes it safer to handle in factories. pMDI also offers a wide formulation window when combined with polyols, and it fits refrigerators, boards, and spray foam. High-functionality pMDI cures faster for continuous board lines, while liquid modified MDI and MDI prepolymers solve handling, free monomer, and fogging issues in specific processes.
What blowing agent should a new rigid foam formula use
Design new formulas around pentane or HFO. Cyclopentane is the mainstream agent for refrigerators and freezers, with mature equipment but flammability that needs explosion-proof design. n-Pentane and isopentane boil lower and can be blended with cyclopentane to optimize cell structure. HFO-1233zd(E) is near-zero GWP, non-flammable, and already scaled in refrigeration and high-end building materials. Avoid HCFC-141b for new projects because it is being phased down under the Kigali Amendment.
What is the difference between water blowing and pentane blowing
Water is a chemical blowing agent: it reacts with NCO to generate CO2, at the lowest cost with zero ODP and GWP. But CO2 conducts heat well and raises embrittlement risk, so water is usually blended with a physical blowing agent in semi-water systems. Pentane is a physical blowing agent with moderate lambda and proven cold chain equipment. Pentane needs explosion-proof design because it is flammable, while water adds no flammability risk but may need help with cell size and strength.
Which catalyst balances gel and blow in rigid foam
TEDA, known as A-33 and usually supplied as a 33 percent solution in dipropylene glycol, is the classic rigid foam catalyst that promotes both gel and blow. It has broad compatibility and appears in almost every rigid foam system formulation. DMCHA and PMDETA lean toward gel for fast demold, while DMEA leans toward blow and improves cell opening. T-12 organotin delivers extreme gel efficiency at tiny doses, but watch the regulatory trend on organic tin. Potassium and quaternary ammonium salts are reserved for trimerization in PIR systems.
What is T-12 and why is it under regulation pressure
T-12 is dibutyltin dilaurate, an organotin catalyst with extremely high gel efficiency in rigid foam. A tiny dose speeds up gelation a lot, so formulators use it to tune the gel-blow balance. The reason for regulation pressure is the broader restriction trend on organotin compounds over health and environment concerns. Formulators facing limits often shift to amine catalysts or adjust the catalyst blend instead.
How much TCPP is used in B1 grade rigid foam
TCPP is the most used additive flame retardant in rigid foam, with low viscosity and good compatibility with polyols. B1 grade formulas typically use 8 to 15 percent TCPP. The caveat is the halogen controversy and the migration risk of additive flame retardants. For better results, formulators combine additive TCPP with reactive phosphorus polyols, which bond phosphorus into the chain and do not migrate or exude.
What makes PIR boards more heat resistant than PUR
PIR boards use a high isocyanate index, usually 200 to 400, with excess pMDI and trimerization catalysts such as potassium salts or quaternary ammonium salts. The reaction pre-builds isocyanurate rings into the polymer network, which raises heat resistance to 140 degrees Celsius and above and improves flame retardance. PUR systems use lower indexes and do not build the same isocyanurate content, so PIR suits stricter fire standards and higher temperature service.
Do flame retardants affect foam cell structure
Yes. Flame retardant loading changes viscosity, cell nucleation, and foam stability, so high doses can coarsen cells or promote collapse. Expandable graphite, for example, needs care at the cell interface because its particles sit between polymer and cell wall. Melamine powder also needs good dispersion to avoid cell defects. The usual fix is to match the surfactant system to the flame retardant package and keep the loading inside the proven window.
Can expandable graphite replace TCPP
Not one for one. Expandable graphite works by expanding into an insulating char layer when heated, while TCPP acts in the condensed and gas phases as a phosphorus flame retardant. Expandable graphite is halogen-free, suppresses smoke, and reaches grades such as DIN 4102 B1 at 8 to 15 percent loading, but it must solve the cell-interface problem. Formulators more often combine expandable graphite or melamine with TCPP to get P-N synergism and better smoke suppression than TCPP alone.
What filler raises compression strength of rigid foam
Glass fiber and wollastonite are the two inorganic fillers used for this purpose, typically added at 5 to 20 percent. They raise compression strength and dimensional stability while lowering thermal expansion, which suits structural board and imitation wood products. The tradeoff is higher viscosity and more equipment wear. Mold release agents are a separate additive family that decides demold integrity and surface quality for molded parts such as refrigerator liners and pipe shells.