In NIR direct-write 3D printing, cure speed is not the only factor. PETMP, a primary thiol, cures faster and converts more double bonds than PE1, a secondary thiol. Yet the team selected PE1 for the printing ink because it stays stable during dispensing and extrusion. PETMP-based ink began gelling near 40 degrees C; PE1-based ink held to about 80 degrees C. Processing stability beats raw cure speed here.
Why this question matters
Thiol-ene curing matters for one practical reason: it beats oxygen inhibition. In a radical cure, oxygen grabs radicals at the surface and stalls the reaction. A thiol can donate hydrogen to a peroxyl radical and form a thiyl radical that gets the chain reaction going again, so curing proceeds even in air. PETMP does this just as well as PE1, so oxygen tolerance is not what sets them apart.
Here is the puzzle: the team measured faster curing for PETMP, then printed with PE1 anyway. Below is why, and what it means for formulators choosing thiols for UV or NIR curing inks.
The two materials under test
| Item | PETMP / TTT | PE1 / TTT |
| Thiol class | primary | secondary |
| Thiol functionality | 4 thiol groups | 4 thiol groups |
| Allyl monomer | TTT | TTT |
| Photoinitiator | BAPO | BAPO |
| Cure trigger | NIR plus upconversion particles | NIR plus upconversion particles |
| Polymerization rate | faster | slower |
| Double-bond conversion | over 80 percent | about 75 percent |
| Thermal polymerization onset (DSC, 5 degrees C per minute) | near 40 degrees C | near 80 degrees C |
PETMP and PE1 look similar on a datasheet. Both carry four thiol groups, so both can build a densely cross-linked network with the same allyl monomer. Both were cured with the same photoinitiator, triggered by near-infrared light through upconversion particles. The difference is local chemistry: in PETMP each thiol sits at the end of a short mercaptopropionate arm; in PE1 each thiol sits on a slightly longer mercaptobutyrate arm. That changes how easily the thiyl radical forms and how easily the cured network can restart reacting on its own when it gets warm.
Results: cure rate and conversion
Under identical light intensity, particle loading, and irradiation conditions, PETMP/TTT polymerized faster than PE1/TTT. Depth-resolved double-bond conversion put PETMP above 80 percent and PE1/TTT around 75 percent. Measured by speed and final conversion, PETMP is the winner.
Seven percentage points of conversion sound small, but for a thin printed layer both values are workable. The practical question is not which resin cures harder in a cuvette; it is which resin survives the path from bottle to printed line.
The thermal test reversed the ranking. In DSC runs at a heating rate of 5 degrees C per minute, PETMP/TTT began thermal polymerization at about 40 degrees C. PE1/TTT did not start until about 80 degrees C.
For a printing ink, 40 degrees C is a real risk. The ink warms in the mixing cup, in the feed line, and inside the nozzle during a long job. A resin that starts cross-linking at 40 degrees C can thicken, clog the nozzle, and lose shape fidelity before printing ends. PE1’s 80 degrees C onset gives a wide processing window. That is why the team selected PE1/TTT for all subsequent direct-write experiments.
Cure speed is therefore not the sole criterion for ink suitability. An ink must survive mixing, delivery, and continuous extrusion without changing its rheology.
Printing performance: silica, speed, strength
| Parameter | Result |
| Fumed silica loadings tested | up to 4 wt percent |
| Optimum fumed silica loading | 4 wt percent |
| Rheology at the optimum | shear-thinning with structural recovery |
| Maximum print speed | 60 mm per second |
| Tensile strength, NIR post-cured direct-write sample | about 55 MPa |
| Tensile strength, mold-cast sample with silica | about 58 MPa |
| Printed structures shown | transparent lattice, black lattice, unsupported spiral |
At four wt percent fumed silica the ink already showed good shear-thinning and structural recovery: it flows under pressure through the nozzle and holds its shape right after extrusion. Adding more silica changes the rheology, but excessive viscosity and yield stress make fast extrusion harder. With the optimized formulation the team printed transparent lattices, black lattices, and unsupported spiral structures. The NIR post-cured printed tensile sample reached about 55 MPa, close to about 58 MPa for the silica-containing mold-cast reference. The 3 MPa gap matters less than it looks: a printed part sees nozzle shear and layer-by-layer buildup that a mold-cast part never does, so preserving nearly all of the reference strength is a strong result. For jigs, lattices, and display structures, that strength is sufficient.
These numbers come from upconversion-particle-assisted NIR curing. Do not transfer them directly to a conventional UV LED coating or ink production line.
What the processing window means step by step
A direct-write job has stages, and the resin must behave at each one. First, mixing: pigments or fillers are stirred in, and the resin sits for minutes to hours before printing. Second, delivery: the ink moves through tubes or a cartridge to the print head. Third, extrusion: pressure pushes the bead through the nozzle, and the resin must thin under shear then thicken again when it stops. Fourth, shape retention: the printed line must hold its geometry until light cures it. Fifth, post-cure: additional exposure raises final conversion and properties.
A resin that gels at 40 degrees C can fail at stage one or two on a warm day or during a long run. PE1, stable to about 80 degrees C, survives all five stages in the tested setup. The trade is lower final conversion, about 75 versus over 80 percent, which the team accepted for process reliability.
Why the team chose the secondary thiol
A 3D printing ink is not a coating that flashes off in seconds. It sits in a cartridge, moves through a feed line, and is extruded bead by bead. A resin that begins reacting at 40 degrees C may gel in the reservoir or nozzle during a long job. PE1, stable to about 80 degrees C, stays liquid until it is printed. The lower final conversion, about 75 versus over 80 percent, was an acceptable trade for process reliability.
This is not an isolated result. A peer-reviewed materials study from 2018 compared several secondary multi-thiols with a primary thiol. At 60 degrees C storage, these systems stayed stable for more than seven days, while the primary thiol system lasted under three days. Such networks have also been used in DLP 3D printing at 50 micrometer vertical resolution. When functionality and molecular structure are comparable, networks of either type can show similar reactivity and material properties. So the stability edge of this chemistry should not be read as proof that it always cures slower; the gap depends on the formula.
Patent activity points in the same direction. A US patent on light-curable thiol compositions was granted in 2026, with filings tracing back to 2017 and publication in 2020. In specific formulations, thiol compositions of this type showed good storage stability alongside PETMP-based ones. A patent protects the compositions it claims; it does not prove industrial-scale manufacturing. Still, it confirms this chemistry is an active choice for UV-curable coatings.
One naming note: the PE1 used in the university study is pentaerythritol tetrakis(3-mercaptobutyrate). A patent mentions a trade-name product, PE1AG, built on the same chemistry, while another material marked PE1 in that patent is a mixture of different thiol esters and is not the study material. Similar codes do not always mean the same resin; check the chemistry before substituting.
Practical recommendations for formulators
- Do not choose a thiol by cure speed alone. Match it to the full printing window.
- For inks that rest in a cartridge or travel through a feed line, weigh thermal stability heavily. It buys time before gelation.
- When the job rewards shape fidelity after extrusion more than peak conversion, make this chemistry the default choice.
- Start fumed silica around four wt percent for shear-thinning. More silica is not automatically better.
- Validate on the actual curing hardware. NIR upconversion results do not predict UV LED line performance.
Limitations
All figures apply to the specific formulations and test conditions in the study. The 40 and 80 degrees C numbers are DSC onsets at a 5 degrees C per minute ramp; they are not long-term storage temperatures. The NIR upconversion system differs from conventional UV LED equipment, so cure depth, speed, and conversion will differ elsewhere. These results describe one formulation family, not a product guarantee or proof of mass production. Readers should also treat the single-digit conversion gap as formulation-specific, not as a universal ranking of the two thiol types.
Bottom line
PETMP cures faster and converts more double bonds than PE1, yet the secondary thiol won the ink slot. PETMP-based ink starts reacting near 40 degrees C, while PE1-based ink stays stable to about 80 degrees C. For direct-write 3D printing inks, the right thiol is the one that survives the printing process, not the one that cures quickest in a test cell.
FAQ
What is the difference between PETMP and PE1?
Both are tetrafunctional thiols with four thiol groups. PETMP is a primary thiol and PE1 is a secondary thiol, meaning the thiol groups sit in different local chemical environments. That difference changes reactivity and thermal stability even though the building blocks look similar.
Why did researchers pick the slower-curing thiol for 3D printing?
PETMP cures faster and reaches over 80 percent double-bond conversion, while PE1 reaches about 75 percent. But PETMP-based ink starts thermal polymerization near 40 degrees C, whereas PE1-based ink remains stable to about 80 degrees C. For an ink that must be mixed, dispensed, and extruded continuously, avoiding premature gelation matters more than peak cure speed.
How stable are the two inks before printing?
In DSC tests at a heating ramp of 5 degrees C per minute, PETMP/TTT began reacting near 40 degrees C and PE1/TTT near 80 degrees C. Those are onset temperatures under a specific test, not storage limits, but they show PE1 gives a much wider safe processing window.
What print speed did the team achieve?
With the optimized ink containing 4 wt percent fumed silica, the fastest printing speed reached 60 mm per second under the study conditions. That speed was measured with the nozzle and formulation used in the study; other nozzles or higher silica loadings will change the practical window.
How strong are the printed parts?
NIR post-cured direct-write printed samples reached about 55 MPa tensile strength, close to about 58 MPa for silica-containing mold-cast reference samples.
What structures did they print?
Transparent lattice structures, black lattice structures, and unsupported spiral structures, showing that the ink can hold shape without support material.
Is a secondary thiol always better than a primary thiol?
Not necessarily. When functionality and molecular structure are comparable, networks of either type can show similar reactivity and material properties. The advantage here is thermal stability for ink handling, not a universal speed or strength gap.
Does thiol-ene chemistry help with oxygen inhibition?
Yes. Thiol groups donate hydrogen to peroxyl radicals and generate thiyl radicals that continue the chain reaction, which reduces oxygen inhibition during curing. PETMP has this ability too; it is not exclusive to one thiol type.
Can these results apply to regular UV LED production lines?
No direct transfer. The data come from NIR curing assisted by upconversion particles. Conventional UV LED coating and ink lines will show different cure depth, speed, and conversion behavior.
Why not add more fumed silica to the ink?
More silica changes rheology, but excessive viscosity and yield stress make fast extrusion difficult. Four wt percent was found to give good shear-thinning and structural recovery without hurting print speed.