Four grades. One styrene maleic anhydride copolymer backbone. What separates them is a single monomer, and that one change sends each grade off to solve a completely different headache.
Here’s the short version. If the problem is pigment that won’t stay dispersed, you want the cationic quaternary ammonium grade. If the problem is antistatic performance that dies after three washes, you want the zwitterionic betaine grade. If the problem is a V-0 rating you can only hit by loading so much flame retardant that the tensile strength collapses, you want the phosphorus grade. If the problem is a dielectric constant that won’t come down while the glass transition temperature won’t come up, you want the imide grade.
One more thing before the details. All four are tunable. Monomer ratios, molecular weight, functional group content, all of it can move to match a specific resin or a specific test somebody has to pass. What shows up on the bench is a place to start, not a locked recipe.
On this page
- Why the styrene maleic anhydride backbone is the starting point
- What styrene maleic anhydride copolymer modification actually changes
- The cationic quaternary ammonium grade
- The zwitterionic betaine grade
- The phosphorus modified grade
- The imide modified grade
- Why a quaternary copolymer instead of four separate additives
- Charge matching, pH windows and processing limits
- How to pick a grade and run a first trial
- Limitations and what still has to be tested
- Bottom line
- Frequently asked questions
Why the styrene maleic anhydride backbone is the starting point
Styrene maleic anhydride has been earning its keep in coatings, plastics and paper for decades, and the reason is that the two monomers cancel out each other’s weaknesses.
Styrene brings rigidity, water resistance and aromatic character, which is what lets the molecule sit comfortably inside styrenic, acrylic and aromatic resin systems instead of fighting them. Maleic anhydride brings polarity, and something better than polarity: a reactive anhydride ring. That ring is the useful part. Open it with water and you get a diacid. Open it with an alcohol and you get a half ester. Feed it an amine and you get an amide or an imide. Give it an epoxide and you get an ester. That single reactive handle is why this backbone has done duty as a pigment dispersant, a compatibilizer, a leveling agent, a sizing agent and a curing agent over the years.
Then you run into the ceiling.
Workable grades, meaning grades that aren’t a nightmare to handle, sit at an anhydride content where polarity is enough to grab onto a pigment particle but not enough to drive real ionic behavior. That same ceiling rules out serious flame retardant chemistry, and it rules out a high thermal limit. Crank the anhydride content up to fix that and the polymer starts behaving differently in other ways, water sensitivity among them.
The other limit is simpler. The backbone does one job. A grade disperses, or it compatibilizes. It doesn’t do both, and it certainly doesn’t also resist flame or hold together at 250 degrees Celsius.
So you introduce a fourth monomer. Change which one, and you change what the product is for.
What styrene maleic anhydride copolymer modification actually changes
Put a fourth monomer into a styrene maleic anhydride copolymer and four things move at once. The charge on the chain, which decides what it sticks to and what it curdles with. The flexibility and bulk of the chain, which decides how thick a stabilizing layer it can build around a particle. The reactivity left over for cure, because the anhydride is still free to bond into a film or a fiber. And the thermal ceiling, which decides whether the grade survives a reflow oven or a 200 degree bake.
The four grades are just four different answers to which of those matters most.
| Grade | Fourth monomer and functional group | What it delivers | Where it usually lands |
|---|---|---|---|
| Cationic quaternary ammonium | Quaternary ammonium salt on a C18 methacrylate chain | Permanent positive charge, pigment anchoring, combined electrostatic and steric stabilization | Waterborne coatings and inks, textile antistatic and softening, paper strengthening and sizing, flocculation |
| Zwitterionic betaine | Sulfobetaine or carboxybetaine group | Net neutral charge, wide pH stability, antistatic effect that is bonded in place | Antistatic and soil release textiles, antistatic masterbatch, coatings and adhesives, personal care |
| Phosphorus modified | Phosphate or phosphonate group bonded to the backbone | Condensed phase char formation, halogen free, non-migrating | V-0 flame retardant coatings, halogen free PP PE ABS, flame retardant adhesives, durable flame retardant textiles |
| Imide modified | Imide ring formed by reacting the anhydride with a primary amine | High thermal decomposition temperature, higher glass transition temperature, low dielectric loss | High temperature coatings, electronic packaging, high temperature adhesives, composite interfaces, 5G laminates |
One word of warning about the word quaternary, because it means two things here and the confusion is genuine. In quaternary copolymer it means four monomers on one chain, a tetrapolymer. In the cationic grade it also means the quaternary ammonium cation, where the nitrogen carries four organic groups and therefore a positive charge that never goes away. Those are not the same idea and it’s worth keeping them apart in a technical conversation.
There’s also an abbreviation trap that has derailed more than one meeting. Styrene maleic anhydride and stearyl methacrylate both get shortened to SMA. In this article SMA always means styrene maleic anhydride. The C18 monomer gets written out in full, as stearyl methacrylate or octadecyl acrylate.
| Monomer | Role in the chain | What it changes in the compound |
|---|---|---|
| Styrene | Rigidity, hydrophobicity, aromatic compatibility | Raises the glass transition temperature, improves compatibility with styrenic and aromatic resins |
| Maleic anhydride | Polarity and reactivity | Anchoring to pigments and fillers, adhesion to polar substrates, later conversion to ester, amide or imide |
| Stearyl methacrylate or octadecyl acrylate | C18 alkyl chain | Flexibility, low surface energy, steric stabilization, internal plasticization |
| Fourth functional monomer | Application specific | Sets the charge character, the flame retardancy or the heat resistance |
The cationic quaternary ammonium grade
Cationization is the whole point of this one, and the mechanism is easy to follow.
A quaternary ammonium group is permanently positive. It has no use for protonation, unlike a primary, secondary or tertiary amine, so its charge doesn’t fold up when the pH climbs. In a waterborne system where pH drifts during storage, that distinction is the difference between a product that holds and a product that doesn’t.
Put this molecule in a millbase and the cationic group latches onto the pigment surface, which on most organic and inorganic pigments carries a negative charge. Now every particle wears the same positive charge and they push each other apart. Meanwhile the C18 chain sticks out into the water and adds a second layer of protection, a steric barrier. Electrostatic repulsion plus steric hindrance. That combination is what keeps a grind genuinely stable rather than just dispersed for a week.
Worth a sample when the problem looks like this:
- A waterborne coating or ink where the pigment grind is poor, the letdown separates in the can, or the film gloss just won’t come up. The cationic group anchors to the pigment and the alkyl chain reaches into the water phase.
- Textile finishing for antistatic and softening. The cationic group adsorbs onto the fiber and cuts friction between fibers, which means less static generated and a better hand feel.
- Paper treatment for strength and sizing. The cationic group binds the negative charge on cellulose, so retention goes up and you need less sizing agent to get the same result.
- Water treatment, flocculation and sludge dewatering. Charge density is adjustable, so the same chemistry can be aimed at different turbidity levels.
The short version: this is the pigment dispersant for waterborne coatings, the paper sizing agent that improves retention, and the cationic flocculant for water treatment. Anywhere a positive charge has to sit on a surface, this grade is the direction.
The failure mode is charge conflict, and it isn’t subtle. A cationic polymer meeting an anionic surfactant, latex or dispersant neutralizes it and drops it out of solution. You see grit, specks or a dispersion that collapses. Before a cationic grade goes into a waterborne formulation, every other component’s charge needs checking.
The zwitterionic betaine grade
This one swaps the permanent positive charge for a betaine group, which is a single monomer holding both a positive and a negative charge arranged so the molecule overall is neutral.
That structure does a couple of unusual things. A betaine isn’t pH sensitive the way a cation is, and it doesn’t go looking for trouble with multivalent metal ions the way an anion does, so it holds up across a wide pH range. Formulating becomes easier, because an entire class of incompatibility is simply gone.
The second consequence is the one that sells. A zwitterionic betaine is chemically bonded into the fiber or the resin. Conventional antistatic agents don’t work that way. They bloom to the surface, soak up atmospheric moisture and bleed charge away through that water film. Which is fine on day one and useless after five laundry cycles, because the migrating molecule has left the building. A bonded betaine group has nowhere to migrate to. The antistatic performance belongs to the material, not to a surface film that can be washed off.
Where it earns its place:
- Textile auxiliaries for antistatic, soil release and easy-clean finishing, when the customer specification says antistatic performance must not decay after repeated washing. The zwitterionic group handles the durable antistatic side, the C18 chain handles the hydrophobic soil release side.
- Coatings and adhesives that need antistatic behavior without giving up adhesion. A zwitterion doesn’t build a charge that repels the substrate, so you don’t pay for conductivity with bond strength.
- Plastic modification as a permanent antistatic masterbatch. Compatibility with polyolefins is good, which is what gets you an evenly dispersed masterbatch instead of a blotchy one.
- Personal care, as a conditioning or thickening agent, where the zwitterionic structure is comparatively kind to skin and eyes.
The short version: this is the permanent antistatic agent that does not wash out, and the additive of choice where a system has to stay stable across a wide pH range.
Watch the isoelectric point. There’s a pH where the positive and negative charges on a zwitterion exactly cancel, net charge hits zero, and solubility bottoms out. Formulate away from that pH or pin the pH with a buffer. The window is broad enough that this usually means shifting a pH unit or two, not redesigning the product.
The phosphorus modified grade
Add a phosphorus-containing flame retardant group to the backbone and you get chemistry that works nothing like a halogen.
Heat a phosphorus compound and it breaks down into polyphosphoric acid. That acid pulls water out of the surrounding polymer, which drives char formation, and char does the actual work: it blocks heat, blocks oxygen, and cuts off the fuel supply reaching the flame. Halogen flame retardants mostly work in the gas phase instead, scavenging the radical species that keep combustion going. Efficient, but you pay for it in acid gas, smoke and toxicity, which is why tightening regulation has pushed the industry toward phosphorus.
The part that makes this grade different from every phosphorus additive on the shelf is where the phosphorus sits. It’s bonded to the SMA backbone. An additive flame retardant mixed into a compound slowly works its way to the surface, blooms, and leaches out in service or in the wash, and the rating quietly decays with it. A bonded phosphorus group is part of the chain. Nowhere to migrate to. Nothing to bloom. Nothing to wash out.
Where it matters:
- Flame retardant coatings where V-0 isn’t being met, or is met only at a loading that wrecks the film. A reactive flame retardant of this kind can reach the rating at a lower addition level and leave the film intact.
- Halogen free flame retardant PP, PE and ABS. Compatibility with polyolefins is good, the dispersion is even, and you get a lot of flame retardant efficiency per unit of phosphorus.
- Flame retardant adhesives, where a part has to be both flame retardant and stuck. The phosphorus group covers the first requirement, the maleic anhydride covers the second, and they don’t fight each other.
- Durable flame retardant textiles. Bonded phosphorus survives laundering in a way a topical finish does not.
The failure mode is loading against mechanicals. Flame retardant efficiency climbs with phosphorus content right up to the point where film formation, flexibility and tensile strength start sliding. The target is the lowest content that still passes, not the most the formulation will swallow. Finding that optimum takes bench work, because it depends on the system.
The imide modified grade
An imide structure comes from reacting that anhydride ring with a primary amine.
Imide rings are about as thermally stubborn as polymer chemistry gets. Fully aromatic polyimides hold long term service temperatures of 250 to 300 degrees Celsius, with short excursions up around 500. The reason is a rigid aromatic ring locked into a strongly bonded imide linkage that refuses to come apart until things get genuinely hot. An unmodified SMA copolymer starts falling apart above 200 degrees Celsius, which is exactly the ceiling this grade exists to lift.
Graft imide functionality in and the thermal decomposition temperature jumps, with the glass transition temperature following. The imide structure throws in mechanical strength and electrical insulation as well, and it lowers polarizability, which is what drags the dielectric constant down. That last property is the reason this grade turns up in electronics and not just in high temperature work.
Where it goes:
- High temperature coatings that can’t yellow, chalk or lose adhesion above 200 degrees Celsius. The imide structure carries the thermal load, the long alkyl chain keeps the film hydrophobic and flexible so it doesn’t turn brittle.
- Electronic packaging materials that have to survive reflow soldering and present a low dielectric constant. Imide takes the heat, the SMA backbone supplies the rigidity.
- High temperature adhesives where lap shear at 250 degrees Celsius can’t fall out of spec. Imide holds the rigidity at temperature, maleic anhydride provides the bonding groups.
- Interface treatment for high performance composites. Compatibility with carbon fiber and glass fiber surfaces is good, and the interface doesn’t debond under thermal cycling.
- High frequency copper clad laminates for 5G, where the dielectric constant has to come down and the glass transition temperature has to go up in the same part. Lower polarizability from the imide structure addresses the first, the rigid backbone addresses the second.
The short version: for electronics this is the low dielectric constant material for high frequency laminates, and for assembly it is the high temperature resistant adhesive base that holds its strength at 250 degrees Celsius.
The failure mode is process temperature. Heat resistance tracks the degree of imidization, and a heavily imidized grade needs a hotter process to finish the conversion. Put it in a line with a narrow window and it underperforms, because the reaction never gets there. Match the grade to the process, not the process to the grade.
Why a quaternary copolymer instead of four separate additives
Conventional additives do one thing each. A dispersant disperses. An antistatic agent handles static. A flame retardant handles flame. Every one of them arrives with its own optimum dosage and its own opinions about the other two.
A four-monomer copolymer works on different logic. Several functional groups ride on one chain, so they hit the interface together and stay together. In these grades the split is clean. The C18 ester brings hydrophobicity and flexibility. Styrene brings rigidity and compatibility. Maleic anhydride brings polarity and reactivity. The fourth monomer brings the specific job.
Three things follow from that, and they’re practical rather than theoretical.
There’s nothing to phase separate. Two additives in one can can partition into different phases, or one can shove the other off the pigment surface. Groups on the same chain can’t do either.
Nobody’s fighting over the interface. When several additives want the same pigment or fiber surface, the winner is decided by kinetics, which is a polite way of saying by luck. One molecule carrying several functions removes the contest.
The plant gets simpler. One component means one feed point, one viscosity to match, fewer interactions to chase. Fewer ingredients to declare, too, which matters when regulatory documentation is on the critical path.
One honest caveat, though. A copolymer isn’t automatically the better answer. Separate additives let you tune each function on its own, and if the flame retardant needs doubling, that’s a spreadsheet edit. Move one ratio in a copolymer and everything else moves with it. That trade-off is worth taking when the problem is interfacial and the functions genuinely have to coexist, which is the situation all four of these grades were built for.
Charge matching, pH windows and processing limits
Four constraints govern how these grades behave in a real formulation. Treat them as design rules, not as troubleshooting notes, because every one of them is predictable before anything goes in the pot.
| Situation | What happens | What to do |
|---|---|---|
| Cationic grade plus an anionic wetting agent, latex or dispersant | Charge neutralization and precipitation, visible as specks or grit | Match the charge of the whole system, or switch to a non-ionic surfactant |
| Zwitterionic betaine grade formulated near its isoelectric point | Lowest solubility, possible hazing or separation | Formulate away from the isoelectric point, or hold the pH with a buffer |
| Phosphorus grade pushed to a very high loading | Film formation and mechanical properties decline | Find the minimum loading that reaches the required rating |
| Imide grade used in a narrow processing window | Incomplete imidization and lower than expected heat resistance | Select the imidization level the process can actually reach |
Two of these cause most of the trouble in the field, so they’re worth restating.
Charge matching isn’t a property of the additive. It’s a property of the formulation. A cationic grade shines in a neutral or cationic system and fails in an anionic one, and the failure isn’t a gradual drift. It’s an event. Precipitate shows up shortly after mixing, which at least makes it easy to diagnose.
The isoelectric point of a betaine is a fixed characteristic of the monomer. Measure it once and the formulation pH just has to stay away from it. Because the solubility curve is broad on both sides of the minimum, a unit or two of pH movement is normally all it takes.
How to pick a grade and run a first trial
Pick from the test the customer has to pass, not from the chemistry. The chemistry follows the failure.
| The problem on the line | Grade to trial | First thing to measure |
|---|---|---|
| Pigment dispersion poor, storage separates, gloss low in a waterborne coating | Cationic quaternary ammonium | Grind fineness, viscosity drift over four weeks, 60 degree gloss |
| Antistatic effect fades after a few washes | Zwitterionic betaine | Surface resistivity before and after laundering |
| V-0 fails, or only passes at a loading that destroys tensile strength | Phosphorus modified | UL 94 rating at the lowest loading that passes, plus tensile strength |
| Dielectric constant too high and glass transition temperature too low on a 5G laminate | Imide modified | Dielectric constant and dissipation factor at the operating frequency, plus glass transition temperature |
Said the way it gets said in a meeting: the formulator with a waterborne coating and a dispersion problem gets the cationic grade. The one with a premium fabric spec and antistatic that washes out gets the betaine grade. The one with a compound that refuses V-0 unless the loading destroys the mechanicals gets the phosphorus grade. The one with a laminate where the dielectric constant won’t drop and the glass transition temperature won’t rise gets the imide grade.
Plan the trial around measured endpoints rather than impressions. Reference standards are what make results comparable between labs, and between suppliers.
| What you are claiming | Test to reference |
|---|---|
| Flame retardancy rating | UL 94 vertical burn, with limiting oxygen index by ASTM D2863 as supporting data |
| Antistatic performance | Surface resistivity by ASTM D257 or ISO 3915 |
| Durability of a textile finish to laundering | AATCC 135 or ISO 6330 |
| Glass transition temperature | ASTM D3418 or ISO 11357 |
| Thermal stability and decomposition onset | Thermogravimetric analysis |
| Dielectric properties | ASTM D150, or IPC-TM-650 procedures for laminate work |
| Bond strength after heat ageing | Lap shear on the bonded joint, measured after ageing |
Limitations and what still has to be tested
Everything above describes mechanisms. Four constraints bound how far those mechanisms will carry.
The windows in the next table come from public polymer science and exist for screening. They are not datasheet values for any specific product and they should never be pasted into a purchase specification.
| Parameter | Typical starting window | Note |
|---|---|---|
| Maleic anhydride content in the backbone | About 10 to 50 percent by weight | Low anhydride content favors compatibility and flexibility, high favors polarity and water dispersibility |
| Glass transition temperature of the unmodified backbone | About 110 to 170 degrees Celsius | Rises with anhydride content |
| Onset of thermal decomposition, unmodified SMA copolymer | Above 200 degrees Celsius | The gap the imide grade is designed to close |
| Long term service temperature, fully aromatic polyimide | 250 to 300 degrees Celsius | Short excursions to around 500 degrees Celsius |
| Lead free reflow peak temperature | About 245 to 260 degrees Celsius | The driver for packaging grades |
| Target dielectric constant for high frequency laminates | Below about 3.5 | With dissipation factor below about 0.005 at the operating frequency |
| Surface resistivity target for antistatic textiles | 10^9 to 10^11 ohm per square | Wash durability is the difficult part |
| Limiting oxygen index for a flame retardant system | Above 28 percent | A V-0 rating additionally requires passing UL 94 vertical burn |
Beyond those, four things stay genuinely system specific and no amount of reading substitutes for a trial.
Compatibility, optimum loading and the balance between functions depend on the resin, the filler, the substrate and the cure schedule. Every system is a little different and most are a lot different.
Imide performance depends on the degree of imidization actually achieved, which depends on the temperature the customer’s line really runs at, not the temperature printed in a specification.
Flame retardancy in a highly filled or highly crystalline system is almost never delivered by one component. The phosphorus grade is a strong element of a flame retardant package, and the rest of that package still has to be designed.
Regulatory status has to be confirmed for the specific grade and the specific market, whether the requirement comes from food contact rules, textile chemical restrictions such as OEKO-TEX, RoHS, or a customer’s own restricted substances list.
Bottom line
One backbone. Four fourth monomers. Four problems off the desk.
The cationic quaternary ammonium grade is for anything that needs a positive charge on a surface. Pigment dispersion, textile antistatic and softening, paper sizing and strengthening, flocculation and sludge dewatering.
The zwitterionic betaine grade is for antistatic that lasts, soil release, and pH stable systems that ordinary antistatic agents can’t hold together.
The phosphorus modified grade is for halogen free flame retardancy that reaches V-0 without destroying the mechanicals, and for flame retardant performance that doesn’t migrate and doesn’t wash out.
The imide modified grade is for heat resistance, low dielectric loss and strength retention at temperature, from high temperature coatings and adhesives through composite interfaces to 5G laminates.
Each grade answers a specific problem a formulator is already losing sleep over. Where the monomer ratio, the molecular weight or the functional group content needs to shift to fit a particular system, that’s tuning, not a new development project.
Frequently asked questions
What is a styrene maleic anhydride copolymer used for?
Styrene maleic anhydride copolymer is used as a pigment dispersant, compatibilizer, sizing agent, leveling agent and curing agent. The styrene units add rigidity and aromatic compatibility, and the maleic anhydride units add polarity plus a reactive anhydride ring that opens with water, alcohols, amines and epoxides. Adding a fourth functional monomer turns it into a tetrapolymer aimed at one specific job.
How does a cationic quaternary ammonium copolymer disperse pigment?
The quaternary ammonium group carries a permanent positive charge and is pH independent. It adsorbs onto pigment particles, whose surfaces are usually negative, so the coated particles repel each other. The C18 alkyl chain extends into the water phase and adds a steric barrier. Electrostatic repulsion plus steric hindrance holds the grind stable, which shows up as lower viscosity drift, no hard settling and higher film gloss.
Why does a zwitterionic betaine copolymer give antistatic performance that survives washing?
Betaine groups carry both a positive and a negative charge inside the same monomer and stay net neutral. Because the group is bonded into the fiber or resin, the effect does not depend on molecules migrating to the surface. Conventional antistatic agents work by blooming to the surface and absorbing moisture, which is why they fade after a few laundry cycles. A bonded betaine group cannot wash out.
What makes a phosphorus flame retardant copolymer different from an additive flame retardant?
The phosphorus is chemically bonded to the polymer backbone rather than physically dispersed. Additive flame retardants migrate, bloom and leach over time, so the rating can drift down after ageing or washing. A bonded phosphorus group stays in the chain and keeps working. Phosphorus also acts in the condensed phase by forming a char layer, which means no halogen, less smoke and lower toxicity.
How does an imide modified copolymer raise heat resistance?
The imide ring is formed by reacting the anhydride with a primary amine. Imide rings are rigid and thermally stable, which is why fully aromatic polyimides hold long term service temperatures of 250 to 300 degrees Celsius with short excursions to about 500. Grafting that structure onto a styrene maleic anhydride copolymer raises its thermal decomposition and glass transition temperatures well above the unmodified backbone.
Can a cationic copolymer be mixed with anionic additives?
No. A cationic polymer and an anionic surfactant, latex or dispersant neutralize each other and form a precipitate, which appears as specks, grit or a collapsed dispersion. In a waterborne system, check the charge of every other component before adding a cationic grade. If the formulation needs an anionic component, switch to a non-ionic wetting agent or rebalance the charge.
What causes a betaine copolymer to precipitate in formulation?
A zwitterionic polymer has a pH at which its positive and negative charges balance, called the isoelectric point. At that pH the molecule has no net charge, solubility is at its lowest, and hazing or separation can appear. Formulate away from the isoelectric point, or hold the pH with a buffer. The usable window is wide, so moving one or two pH units usually solves it.
How much phosphorus does a flame retardant copolymer need?
There is no single number, because the requirement depends on the resin, the filler loading and the rest of the flame retardant package. The pattern is consistent though. Flame retardancy improves as phosphorus content rises, but past a point the extra phosphorus starts to hurt film formation, flexibility and tensile strength. The right answer is the lowest content that still reaches the required rating.
What dielectric constant can an imide grade reach for 5G laminates?
High frequency laminates commonly target a dielectric constant below about 3.5 with a dissipation factor below about 0.005, and imide modification helps on both counts by reducing polarizability. The exact figure depends on the resin it is blended into, the cure schedule and the measurement frequency, so verify at the frequency your design actually uses rather than trusting one datasheet value.
Which grade should be used for antistatic textiles that survive washing?
The zwitterionic betaine grade. It bonds into the fiber instead of sitting on the surface, so its antistatic effect does not depend on surface migration and does not rinse away. Measure surface resistivity before and after repeated laundering to AATCC 135 or ISO 6330, and compare against the 10^9 to 10^11 ohm per square range that antistatic textiles usually target.
Why use a quaternary copolymer instead of separate additives?
Because separate additives compete for the same interface and can split into different phases in storage. A four-monomer copolymer puts the hydrophobic, rigid, polar and functional groups on one chain, so they reach the pigment or fiber surface together and stay together. That also means one feed point, one viscosity and fewer components to declare. The trade-off is that each function can no longer be tuned on its own.
What should be measured in a first lab trial?
Measure the property you are trying to fix, the way the end use measures it. For a coating that means grind fineness, viscosity drift over four weeks and gloss. For a textile it means surface resistivity before and after laundering. For flame retardancy it means the UL 94 rating at the lowest loading that passes, plus tensile strength. For a laminate it means dielectric constant and glass transition temperature.