A soft grip and a hard clip can come out of the same bag of pellets, which is the first thing worth understanding about thermoplastic elastomer grades. Inside one styrenic SEBS series, tensile strength climbs from roughly 4 MPa at 40 Shore A to 20 MPa at 60 Shore D. Elongation goes the opposite way, from above 600 percent down to 450. Compression set ignores the trend entirely, and that is how ordering one step harder can leave a seal worse than it started.
The soft grip on a power tool, the seal around a door, the liner in a bottle cap, the jacket on a charging cable. Four parts, four different feel, one family. What goes wrong in that family is rarely the polymer. It is usually a row of a datasheet that nobody read.
What a thermoplastic elastomer grade actually is
TPE is short for thermoplastic elastomer. The trade also sells it as thermoplastic rubber, or TPR. None of those names points at a single product. The family splits by chemistry into styrenic, olefinic, polyurethane, polyester, polyamide and vinyl chloride types, and two of those six can differ in price by more than two grades inside either one of them.
Every one of them is built as a two-phase system. Hard segments gather into clusters that behave as physical crosslinks, and the chemistry behind them varies from polystyrene blocks to crystalline PBT to polyurethane hard segments. Soft segments, usually rubber or polyether chains, occupy the space between the clusters and supply the recovery. Warm the material and the hard domains soften enough to flow. Cool it and they reassemble.
That one idea covers both the convenience and the ceiling of the family. Pellets drop into a standard hopper, the melt fills a standard tool, and the cycle runs in seconds.
Grades arrive as natural colored pellets that feel dry, packed in 20 kg or 25 kg bags. The bag says nothing about hardness. That is what the sheet is for.
The six families and why the family comes before the grade
Nobody starts a TPE project by picking a number. The starting point is chemistry, because hardness and flow can be dialed inside a family while heat resistance, oil resistance and the ability to bond are fixed by the family. Rank thermoplastic elastomer grades from different families on hardness alone and the ranking means nothing.
Table 1: the six families.
| Family | Typical structure | Core strength | Main limit | Typical use |
| Styrenic, TPE-S with SBS and SEBS | styrene butadiene styrene or styrene ethylene butylene styrene triblock, with polystyrene blocks acting as the physical crosslinks; SEBS is hydrogenated SBS | softest grades in the family, easiest to overmold, accepts heavy oil extension, low density, no curing residue, food contact possible, SBS is the cheapest route | moderate heat and oil resistance, and the SBS backbone keeps its double bonds so it ages faster than the hydrogenated version | soft touch overmolding, weather seals, toys, cable jackets, medical parts |
| Olefinic, TPO and TPV | TPO is a mechanical blend of EPDM in polypropylene; TPV vulcanizes the EPDM during the blend so cured particles disperse in a polypropylene matrix | weather and ozone resistance, low specific gravity, friendly price; TPV pairs low compression set with thermoplastic processing | TPO is weak on compression set and abrasion; TPV melt viscosity is high and needs large gates and high injection pressure | bumper and impact modification for TPO; glass run channels, seals, edge trim and grips for TPV |
| Polyurethane, TPU | diisocyanate plus polyol plus chain extender, alternating hard and soft segments, in ether and ester types | best abrasion resistance in the family, high strength, strong oil resistance, wide hardness range | ester types hydrolyze, the material is hygroscopic and must be dried, and it costs more than TPE-S | footwear soles, hose, rollers, pneumatic tube, film, wear sleeves |
| Polyester, TPEE | crystalline PBT hard segments with polyether or polyester soft segments, a multiblock copolymer | rubber elasticity with engineering plastic strength, plus heat, fatigue and oil resistance | high price keeps it out of general use | hydraulic hose, high and low temperature cable jacket, drive belt, damping parts |
| Polyamide, TPAE | high melting polyamide hard segments such as PA6 or PA66 with amorphous polyether soft segments | highest service temperature in the family, good heat aging and chemical resistance, fills the gap between TPU and silicone | high price, a narrow processing window, few grades on the market | automotive fuel line and harness jacket, hot melt adhesive, metal powder coating |
| Vinyl chloride, TPVC | high polymerization degree PVC, partly crosslinked or blended with NBR to gain elasticity | an extension of flexible PVC with better compression set, flame retardant, mature coloring and extrusion, good value | contains halogen, which brings environmental and recycling pressure, and weather resistance sits below the olefinic types | automotive window seals, glass channels, construction gaskets, hose and cable cover |
Three of them stay qualitative here. The olefinic blends, the polyester types and the polyamide types have textbook coverage available rather than grade level sheets, so the honest move is to leave the numbers out instead of borrowing them from a cousin. The styrenic family carries the rest of the article, being the biggest by volume, the most used in overmolding and the easiest to enter.
Physical crosslinks and the trade you cannot escape
Cured rubber hangs together on chemical crosslinks made with sulfur or peroxide, and once those form there is no way back. That is why rubber scrap ends up as filler. A TPE hangs together on physical crosslinks instead, and nearly every processing advantage the family has flows from that one difference.
No mixing. No curing vessel. A standard injection machine or extruder. Seconds per cycle instead of minutes. Sprue, runner and trim that can go back through the barrel more than once. For a molder moving work off rubber, that list is the whole argument for thermoplastic elastomer grades.
It is also the whole limitation. Physical crosslinks relax under sustained heat or sustained load, so heat resistance, oil resistance and resistance to permanent deformation all land below a well cured compound. Ask a part to hold a seal at 100 degrees Celsius for years and you are asking the structure to do the one thing it cannot.
How to compare thermoplastic elastomer grades inside one series
One styrenic series keeps the same formulation framework and moves two dials: how much oil goes in, and the ratio of resin to oil. Hardness travels the whole range without the chemistry changing. Five grades from one European SEBS compounder show the range, and because a single supplier made all five, the comparison is cleaner than anything assembled from a catalog.
Table 2: the hardness ladder inside one series.
| Grade position | Tensile strength (MPa) | Elongation at break (percent) | Tear strength (N/mm) | Compression set at 23 and 70 C (percent) | Density (g/cm3) |
| 40 Shore A | 4 to 4.5 | above 600 | 8 | 18 and 36 | 1.08 |
| 60 Shore A | 6 | 650 | 18 | 21 and 46 | 1.16 |
| 80 Shore A | 8.5 | 630 | 28 | 33 and 56 | 1.17 |
| 90 Shore A, also quoted as 35 Shore D | 11.5 | 600 | 32 | 20 and 40 | 1.17 |
| 60 Shore D | 20 | 450 | 50 | not published | 1.15 |
Four readings follow from that table, and three of them run against the habit of treating hardness as a stand-in for everything else.
- Strength and tear travel together. Tensile runs from 4 to 4.5 MPa at the soft end up to 20 MPa at the hard end, and tear runs from 8 to 50 N/mm across the same span. A harder grade is tougher, and it wears better.
- Elongation drops, but not from the bottom of the range. The peak sits at 650 percent on the 60 Shore A grade, and the 40 Shore A is only quoted as above 600. Stretch does not follow hardness either.
- Density is not monotonic. It reads 1.08, 1.16, 1.17, 1.17 and then 1.15 at 60 Shore D, because filler and oil ratios move by grade. Interpolating part weight from hardness will be wrong.
- Compression set is not monotonic either. At 23 degrees Celsius the series reads 18, 21, 33 and 20 percent, and the hard end publishes nothing at all. The 80 Shore A grade is the worst of the four, which no hardness ordered table would predict.
What one 80 Shore A datasheet contains
80 Shore A carries more traffic than any other band among thermoplastic elastomer grades. It feels like rubber and still resists collapsing under assembly load. Below is a complete sheet for one grade in that band, run to DIN and ISO methods.
Table 3: a full 80 Shore A sheet.
| Property | Test method | Unit | Value | Note |
| Hardness | DIN ISO 48-4 | Shore A | 80 | balance point between soft touch and load bearing |
| Density | ISO 1183 | g/cm3 | 1.17 | includes filler and oil, heavier than a plain SEBS base |
| Tensile strength | DIN 53504 | MPa | 8.5 | measured lengthwise at 200 mm per minute |
| Elongation at break | DIN 53504 | percent | 630 | stretches far, so a snap fit does not tear |
| Tear strength | DIN ISO 34 | N/mm | 28 | controls whether an overmolded edge lifts |
| Compression set at 23 C for 72 h | DIN ISO 815-1 | percent | 33 | the headline claim of the grade |
| Compression set at 70 C for 24 h | DIN ISO 815-1 | percent | 56 | the row a seal has to be judged on |
| Overmolding substrate | datasheet statement | none | polypropylene | two shot work on a PP frame |
| Melt temperature | supplier recommendation | degrees Celsius | 190 to 220 | narrow window, do not run it like polypropylene |
| Mold temperature | supplier recommendation | degrees Celsius | 20 to 40 | cold mold, fast setting, short cycle |
| Drying | supplier recommendation | degrees Celsius and hours | 80 for 3 to 4 | moisture below 0.02 percent |
| Abrasion loss, resistivity and flame class | DIN ISO 4649, IEC 62631, UL94 | mm3, ohm-cm, class | not published | pick another grade if these are needed |
Two cautions come with those numbers. They were measured on uncolored material, and the sheet itself calls them reference values rather than a specification, so geometry, color and process conditions all shift them. Three rows also read as not published: abrasion loss, volume and surface resistivity, and flame class. A part that depends on any of the three is looking at the wrong grade rather than at a hole in the sheet.
Four datasheet rows that decide whether the part works
Most of a sheet is background. Four rows decide what happens in the field, and they are seldom the rows a buyer checks first.
Table 4: the four rows that decide.
| Datasheet row | What it decides | What fails when it is skipped |
| Overmolding substrate | which base resin the grade was compounded to bond to | the soft layer peels off the frame at the interface |
| Compression set at 70 C | how much sealing force survives heat | the seal takes a permanent set and leaks after thermal cycling |
| Tear strength | whether a nick grows into a split | the edge of a grip tears away in handling |
| Melt temperature window | where the melt flows without degrading | short shots at the low end, oil bleed and odor at the high end |
The overmolding row is where projects die. The sheet names the base resin the grade was built to stick to. No amount of tuning turns a polypropylene bonding grade into a nylon bonding grade, because the interface either forms or it does not.
The 70 degrees Celsius set row is where warranties die. A seal picked on the 23 degrees Celsius figure can look superb on paper and still take a permanent set after a few thermal cycles. In this grade the number roughly doubles between the two test temperatures.
Hardness does not predict compression set
Sort the five grades by hardness and compression set breaks ranks. At 23 degrees Celsius the 40 Shore A grade reads 18 percent, the 80 Shore A reads 33, and the 90 Shore A returns to 20. At 70 degrees Celsius the same three read 36, 56 and 40. The softest of the three holds a seal better than the middle of the range does.
The driver is formulation. Oil content, the molecular structure of the SEBS base and the rest of the recipe set the value, and all three can move while the hardness target stays put. Hardness sets the feel. The recipe sets the set.
Which is why the most common mistake in this family is mechanical rather than analytical. A seal leaks, so somebody orders the next hardness step up. The feel of the part changes, the shrinkage changes, the bond at the interface changes, and the failure mode that started the conversation is still there.
The grade table by duty
Sorted by job rather than by hardness, TPE grades fall into nine groups. Each carries its own set of published values.
Table 5: grades grouped by duty.
| Duty band | Supplier type | Representative grade | Key published values |
| Softest grip | European SEBS compounder | 40 Shore A injection grade, low odor, bonds to polypropylene | density 1.08 g/cm3, tear 8 N/mm |
| General purpose | European SEBS compounder | 60 Shore A grade, bonds to polypropylene | MVR 10 cm3 per 10 min at 235 C and 5 kg, UL94 HB at 1.5 mm, tear 18 N/mm |
| General purpose | European SEBS compounder | 80 Shore A grade, improved set, bonds to polypropylene | density 1.17 g/cm3, tear 28 N/mm, set 33 percent at 23 C |
| Wear band | European SEBS compounder | 90 Shore A grade quoted as 35 Shore D, injection | tear 32 N/mm, tensile 11.5 MPa |
| High hardness | European SEBS compounder | 60 Shore D grade, bonds to polypropylene | tensile 20 MPa, tear 50 N/mm, volume resistivity 1.0E15 ohm-cm |
| Polyamide bonding, two shot | European SEBS compounder | 60 Shore A 2K grade for PA6 and PA66 | melt 220 to 250 C, mold 60 to 80 C, dry 80 C for 3 to 4 h |
| Flame retardant | European SEBS compounder | 90 Shore A grade certified to UL94 V-0, bonds to polypropylene | density 1.29 g/cm3 |
| Closure gasket | Southeast Asian olefinic TPE producer | 95 Shore A grade for continuous compression molding, EU 10/2011 and 21 CFR 177.1210 | specific gravity 0.93, tensile 147 kgf/cm2, elongation 652 percent |
| Closure gasket | Southeast Asian olefinic TPE producer | 88 Shore A non PVC grade, extrusion | specific gravity 0.90, elongation 682 percent, extrusion 150 to 200 C |
| Sealing TPV | Global TPV producer | 69 Shore A TPV grade | brittleness -60 C, continuous service 135 C, FMVSS 302 |
| Hard wear TPV | Global TPV producer | 93 Shore A TPV grade, recyclable | brittleness -54 C, continuous service 135 C |
| Polyamide bonding TPV | Global TPV producer | 85 Shore A 2K TPV grade | bonds PA6 and PA66, fatigue and UV resistant, mold temperature close to nylon |
Where each family actually ships
Two shot overmolding is the center of gravity for the styrenic family. A rigid plastic frame carries structure, the TPE carries grip and seal, and one part leaves the press with two materials in it. The rest of the map is settled by heat, oil and food contact, and one of those three usually picks among thermoplastic elastomer grades before anyone compares a number.
Table 6: application areas.
| Application area | Typical parts | What the grade has to carry |
| Overmolding and two shot | power tool and appliance grips, toothbrush handles, razors, automotive interior parts | the datasheet substrate row first, since PP takes a standard grade and PA6 or PA66 needs a 2K grade |
| Sealing and construction | window seals, glass channels, curtain wall gaskets, appliance door seals | compression set and weather resistance, with SEBS or TPV for long outdoor life and no SBS |
| Soft touch parts | phone and earphone cases, wrist straps, mice, remote control keys | the 40 to 60 Shore A band, plus moisture and color control on light parts to stop oil bleed |
| Toys and consumer goods | soft toy parts, pencil grips, sports guards, yoga mats | a SEBS base, food contact capability and a compliance statement for children’s articles |
| Cable and electrical | low voltage cable jacket, earphone cable, charging pile sleeve, flame retardant jacket | a halogen free replacement for flexible PVC, and a certified flame retardant grade rather than additives in a standard one |
| Automotive | glass run channels, seals, dust boots, harness jacket, floor mats | heat and oil resistance, which pushes most of it to TPV and TPEE, with TPE-S held to interior and soft touch work |
| Medical and food contact | infusion tube, medical hose, gloves, stoppers, closure and crown cap liners | no double bond residue, so SEBS rather than SBS, plus full migration and heavy metal documentation for the exact grade |
Processing settings that travel with the grade
Six settings account for most processing complaints about thermoplastic elastomer grades. The first is the cheapest to get right.
- Dry first. A styrenic TPE picks up less water than polyamide or polyurethane, but sheets still ask for 80 degrees Celsius for three to four hours and moisture under 0.02 percent. Light and natural grades that skip it come out streaked with silver and dotted with bubbles.
- Melt at 190 to 220 degrees Celsius with the mold at 20 to 40. That window is narrow on purpose, and the cold mold is deliberate, since fast setting is what keeps the cycle short.
- Re-set everything for a polyamide bonding grade. Those want 220 to 250 degrees Celsius melt and 60 to 80 degrees Celsius mold, and a mold colder than that will not build a bond however long you pack it.
- Budget for shrinkage above polypropylene and ABS. Less hardness means more oil, and more oil means more shrink. Long parts, thin walls and tight dimensional chains need allowance in the tool plus correction on trial.
- Design around shear thinning. Viscosity falls fast as shear rate climbs, so put gates and runners on the high shear side, inject faster and hold back pressure down to avoid hesitation and weld lines.
- Cap the regrind. Reuse beats cured rubber hands down, but every extra pass adds color drift, odor and degradation, so the share of regrind in the shot needs a number and that number needs to hold.
Four failure modes worth memorizing
Most field complaints about thermoplastic elastomer grades fall into four patterns.
- A styrene butadiene grade on an outdoor part. The backbone double bonds go first, and the part hardens and crazes. A hydrogenated SEBS base fixes it, and nothing else does.
- A standard styrenic grade overmolded on polyamide or polycarbonate. No bond forms at the interface and the soft layer peels off under peel load. Only a 2K grade with matched melt and mold temperatures works.
- A styrenic TPE used as a drop-in for flexible PVC. Oil and solvent resistance is the soft spot in this family, and grease contact swells the part and drains its strength. Run an immersion test before the drawing, not after.
- Melt above the window, or a long dwell in the barrel. Oil migrates to the surface, the part goes tacky, odor climbs and the color drifts.
Limitations
- Three of six families stay qualitative. For the olefinic blends and the polyester and polyamide types the source material stops at textbook level, and inventing grade data would be worse than showing the gap.
- These numbers describe one series from one supplier. Another compounder’s ladder will have the same shape and different digits. The shape transfers, the digits do not.
- Datasheet values are reference values. They come off uncolored plaques, and a colored production part will not match them exactly.
- Nothing here covers long term aging, low temperature brittleness or flex fatigue for the styrenic series. If an application depends on those, it needs its own validation.
- The account of the non-monotonic compression set is a mechanism the formulation implies, not something that was measured. Treat it as a reason to check a row, not as a model.
Bottom line
Thermoplastic elastomer grades are a ladder in strength and a scatter everywhere else. Tensile and tear climb with hardness, and that much is safe to design against. Compression set, density and elongation do not climb, and those three decide whether the seal seals, whether the part weighs what the drawing says, and whether the clip survives assembly. Read the duty row first, read the 70 degrees Celsius set row second, then order the sample.
FAQ
What is the difference between TPE and vulcanized rubber
Vulcanized rubber is held together by chemical crosslinks built with sulfur or peroxide, and those bonds cannot be undone once they form. A thermoplastic elastomer uses physical crosslinks instead, where hard segments cluster into domains that soften on heating and re-form on cooling. The practical result is that TPE needs no mixing step and no curing vessel, runs on standard injection and extrusion equipment, and accepts regrind. The trade is heat and oil resistance, plus worse compression set under sustained load.
Which grade should I start with for a soft grip
Start in the styrenic family between 40 and 60 Shore A. That band gives the rubber feel buyers expect while still holding shape under assembly load, and it is where overmolding grades for polypropylene are most abundant. If the part also has to survive outdoor light or long hot cycles, move to a hydrogenated SEBS base rather than staying on a styrene butadiene base. Confirm the substrate row on the sheet before ordering anything.
Why does compression set rise and then fall across the hardness ladder
Compression set follows oil content, the molecular structure of the SEBS base and the rest of the formulation, not hardness. The softest grade in a series carries the most extension oil, and the hard end carries a different balance again, so the value cannot be read off the hardness number. In one series the 40 Shore A grade returns 18 percent at 23 degrees Celsius against 33 percent for the 80 Shore A grade. Only a sheet row settles it for a specific grade.
Can a standard TPE-S grade bond to polyamide
No. A standard styrenic grade is formulated to bond to polypropylene. On polyamide 6 or polyamide 66 the interface forms no effective bond and the two materials separate under peel. Bonding to nylon needs a dedicated 2K grade whose melt and mold temperatures are raised to match the substrate, typically 220 to 250 degrees Celsius melt and 60 to 80 degrees Celsius mold. The same rule applies to polycarbonate.
What does an 80 Shore A datasheet actually tell you
It gives a reference profile, not a specification. A typical sheet lists hardness 80 Shore A by DIN ISO 48-4, density 1.17 g/cm3 by ISO 1183, tensile strength 8.5 MPa and elongation 630 percent by DIN 53504, tear strength 28 N/mm by DIN ISO 34, and compression set of 33 percent at 23 degrees Celsius and 56 percent at 70 degrees Celsius by DIN ISO 815-1. Values are measured on uncolored material and shift with part geometry, color and processing.
How do you read the overmolding row on a TPE datasheet
Look for the substrate named rather than for a yes or a no. Sheets state the base resin the grade was compounded to adhere to, for example polypropylene or polyamide 6 and 66. A grade that names polypropylene will not hold on nylon however the process is tuned. Three conditions decide whether the stated bond happens: a clean substrate surface, a mold temperature high enough to soften the interface, and adequate packing pressure.
Does a harder grade always seal better
No, and this is the most expensive assumption in the family. Hardness sets feel and load bearing. Sealing depends on compression set, which is set by oil content and formulation. In one series the 40 Shore A grade returns 18 percent set at 23 degrees Celsius, the 80 Shore A returns 33 percent and the 90 Shore A returns 20 percent. A harder grade from the same supplier can seal worse than the softer one.
What drying condition does a SEBS compound need before molding
A styrenic TPE absorbs less water than polyamide or polyurethane, but its sheet still calls for drying at 80 degrees Celsius for three to four hours and a moisture level below 0.02 percent. Light and natural grades are the ones that punish a skipped step. The visible result is silver streaking and bubbles on the surface, and the fix afterwards is a full regrind cycle that wastes the run.
How much shrinkage should a TPE mold be allowed for
More than polypropylene or ABS, and more at lower hardness. Shrinkage grows as oil content rises, so a 40 Shore A grade moves further than a 60 Shore D grade from the same series. Long parts, thin walls and tight dimensional chains all amplify the error. The workable approach is to leave generous allowance in the tool and correct on trial rather than to size the cavity from one shrinkage figure.
Can TPE regrind be reused
Yes, and repeated reuse is a genuine advantage over vulcanized rubber, where scrap becomes filler. Most thermoplastic elastomer grades tolerate regrind as long as the share stays capped. Each pass through the barrel does degrade the material, though: color drifts, odor rises and mechanical values fall. Set a ceiling for the share of regrind in the shot and hold it, because a recipe that drifts upward quietly is what turns a stable process into a color and smell complaint six months later.
Which family should be used for outdoor weather exposure
Olefinic types, meaning TPO and TPV, lead on weather and ozone resistance, and TPV also holds compression set close to a cured rubber. Inside the styrenic family the hydrogenated SEBS base survives outdoor exposure while the styrene butadiene base does not, because its backbone still carries double bonds that age first. Long life outdoor parts should not be specified on a styrene butadiene grade at all.
Is TPE food contact approved by default
No. Approval belongs to a specific grade under a specific regulation, not to the family. A closure gasket grade may carry a declaration for a European plastics regulation and a United States food additive regulation while a neighboring grade in the same catalog carries neither. Ask for the migration and heavy metal documentation for the exact grade, and treat any general statement about the material class as no evidence at all.